Celanese VECTRA S471 LCP, 45% Mineral / Glass Reinforced
Categories:
Polymer
;
Thermoplastic
;
Liquid Crystal Polymer (LCP)
;
Liquid Crystal Polymer (LCP), 50% Glass Fiber Filled
Material Notes:
High flow, High Heat resistance, Low Warpage, for Thick Walled (>0.2mm) or thin (<0.2mm)& Thick Walled combination parts.
Information provided by Celanese
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.76
g/cc
0.0636
lb/in³
ISO 1183
Linear Mold Shrinkage, Flow
0.0020
cm/cm
0.0020
in/in
ISO 294-4
Linear Mold Shrinkage, Transverse
0.0050
cm/cm
0.0050
in/in
ISO 294-4
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
120
MPa
17400
psi
5mm/min; ISO 527-2/1A
Elongation at Break
1.4 %
1.4 %
5mm/min; ISO 527-2/1A
Tensile Modulus
12.0
GPa
1740
ksi
50mm/min; ISO 527-2/1A
Flexural Strength
185
MPa
26800
psi
ISO 178
Flexural Modulus
12.0
GPa
1740
ksi
ISO 178
Flexural Strain at Break
2.0 %
2.0 %
ISO 178
Izod Impact, Notched (ISO)
8.00
kJ/m²
3.81
ft-lb/in²
ISO 180/1A
Charpy Impact Unnotched
1.00
J/cm²
4.76
ft-lb/in²
ISO 179/1eU
Charpy Impact, Notched
0.600
J/cm²
2.86
ft-lb/in²
ISO 179/1eA
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+16
ohm-cm
1.00e+16
ohm-cm
IEC 60093
Surface Resistance
1.00e+11
ohm
1.00e+11
ohm
IEC 60093
Dielectric Constant
4.0
@Frequency 1e+6 Hz
4.0
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor
0.0070
@Frequency 1e+6 Hz
0.0070
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index
200
V
200
V
IEC 60112
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
8.00
µm/m-°C
4.44
µin/in-°F
ISO 11359-2
CTE, linear, Transverse to Flow
17.0
µm/m-°C
9.44
µin/in-°F
ISO 11359-2
Melting Point
350
°C
662
°F
10°C/min; ISO 11357-1,-2,-3
Deflection Temperature at 1.8 MPa (264 psi)
315
°C
599
°F
ISO 75-1, -2
Deflection Temperature at 8.0 MPa
271
°C
520
°F
ISO 75-1, -2
Flammability, UL94
V-0
V-0
Processing Properties
Metric
English
Comments
Processing Temperature
80.0
-
120
°C
176
-
248
°F
cavity
355
-
370
°C
671
-
698
°F
hot runner
Feed Temperature
60.0
-
80.0
°C
140
-
176
°F
Zone 1
330
-
350
°C
626
-
662
°F
Zone 2
340
-
360
°C
644
-
680
°F
Zone 3
345
-
365
°C
653
-
689
°F
Zone 4
355
-
370
°C
671
-
698
°F
Die Temperature
355
-
370
°C
671
-
698
°F
Melt Temperature
360
-
375
°C
680
-
707
°F
Drying Temperature
150
-
170
°C
302
-
338
°F
Dry Time
6.00
hour
6.00
hour
Injection Pressure
50.0
-
150
MPa
7250
-
21800
psi
Hold Pressure
50.0
-
150
MPa
7250
-
21800
psi
Back Pressure
<=
3.00
MPa
<=
435
psi
Descriptive Properties
Injection speed
medium
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Celanese VECTRA S475 LCP, 32% Mineral / Glass Reinforced
Celanese VECTRA S135 LCP, 35% Glass Reinforced
Celanese VECTRA E473i LCP, 32% Mineral / Glass Reinforced
Celanese VECTRA E130i LCP, 30% Glass Reinforced
Celanese VECTRA E471i LCP, 35% Specialty
PHCQ525 / 178980
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.