MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

LyondellBasell Petrothene LT493721 HDPE
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Blow Molding Grade

Material Notes: Petrothene LT493721 exhibits an enhanced balance of stiffness and environmental stress crack resistance. Typical applications include bottles for detergents, household and industrial chemicals. This product is formulated with synthetic antistat. Applications: Bottles For Consumer Goods, Bottles for Industrial Use

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.949 g/cc0.0343 lb/in³ASTM D1505
Environmental Stress Crack Resistance >= 300 hour>= 300 hourASTM D 1693
Melt Flow 0.34 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.34 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6363ASTM D2240
Elongation at Break >= 1330 %>= 1330 %ASTM D638
Flexural Modulus, 1% Secant 1080 MPa157000 psiASTM D790
Tensile Impact Strength 282 kJ/m²134 ft-lb/in²ASTM D1822
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 65.0 °C149 °Funannealed; ASTM D648
Vicat Softening Point 124 °C255 °FASTM D1525
Brittleness Temperature <= -76.0 °C<= -105 °FASTM D746
 
Descriptive Properties
Processing MethodExtrusion Blow Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEQT8843 / 220477

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.