MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Chemlon® 109 U Nylon 66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Unreinforced

Material Notes: Availability: Europe; Asia Pacific; North America

Additive: UV Stabilizer

Uses: Automotive Applications

Automotive Specifications: FORD WSS-M4D666-A2

Form: Pellets

Processing Method: Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.09 g/cc0.0394 lb/in³ISO 1183
Water Absorption 0.80 %
@Time 86400 sec
0.80 %
@Time 24.0 hour
ISO 62
Maximum Moisture Content 0.200.20
Linear Mold Shrinkage 0.015 - 0.020 cm/cm0.015 - 0.020 in/inISO 1183
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 50.0 MPa7250 psiISO 527-2
Elongation at Break 45 %45 %ISO 527-2
Flexural Strength 65.0 MPa9430 psiISO 178
Flexural Modulus 1.70 GPa247 ksiISO 178
Izod Impact, Notched (ISO)  19.9 kJ/m²
@Temperature -40.0 °C
9.50 ft-lb/in²
@Temperature -40.0 °F
ISO 180/A
 94.5 kJ/m²
@Temperature 22.8 °C
45.0 ft-lb/in²
@Temperature 73.0 °F
ISO 180/A
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmISO 1325
Dielectric Strength 16.9 kV/mm
@Thickness 3.00 mm
430 kV/in
@Thickness 0.118 in
ASTM D149
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 52.2 °C126 °FUnannealed; ISO 75-2/A
Flammability, UL94 HB
@Thickness 0.762 mm
HB
@Thickness 0.0300 in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 209 - 285 °C409 - 545 °F
Middle Barrel Temperature 265 - 290 °C509 - 554 °F
Front Barrel Temperature 265 - 295 °C509 - 563 °F
Nozzle Temperature 265 - 285 °C509 - 545 °F
Melt Temperature 270 - 295 °C518 - 563 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ0436 / 236927

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.