MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

(Viewing data as-entered. Click here to return)
Tra-Con Tra-Bond 789-3T3N1 Moisture Resistant Adhesive
Categories: Polymer; Adhesive; Thermoset

Material Notes: TRA-BOND 789-3T3N1 adhesive is a thixotropic version of TRA-BOND 789-3. It is a one component, high strength, toughened adhesive designed for use in applications which require good moisture resistance.

Information provided by Tra-Con Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Viscosity 210000 cP
@Temperature 25.0 °C
Mixed (cp #52, 2.5 rpm)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 874 hrs @ 93°C
Adhesive Bond Strength 4350 psiLap shear, alum to alum, 30 min @ 150°C
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.60e+15 ohm-cm
@Temperature 100 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 68.5 µm/m-°C
@Temperature 25.0 - 65.0 °C
Alpha 1
 195 µm/m-°C
@Temperature 150 - 190 °C
Alpha 2
Maximum Service Temperature, Air 150 °C
Minimum Service Temperature, Air -55.0 °C
Glass Transition Temp, Tg 120 °CUltimate Tg; TMA
 
Processing PropertiesOriginal ValueComments
Cure Time 1.00 hour
@Temperature 125 °C
 30.0 min
@Temperature 150 °C
Shelf Life 12.0 Month
 
Descriptive Properties
Color Blue
Thixotropic Index 4.10.5 rpm/5 rpm; cp #52

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Epoxy Technology EPO-TEK® H63 Thermally Conductive, Electrically Insulating Epoxy
Lord Adhesives CircuitSAF™ ME-456 Epoxy Dam Encapsulant
Overview of materials for Epoxy Adhesive, Flexible
Tra-Con Tra-Bond 789-3TN1 Moisture Resistant Adhesive
Tra-Con Tra-Bond 789-3 Moisture Resistant Adhesive

PTRAC155 / 71083

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.