MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Hexcel® HexPly® M73/IM7 Curing Toughened Epoxy Resin/Unidirectional Tape
Categories: Polymer; Thermoset; Epoxy

Material Notes:

Information provided by Hexcel Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 0.340 ksiIPS Properties ( 45 tension), 150°F/85% RH to equilibrium (approximately 1.1% weight gain)
 0.580 ksiIPS Properties ( 45 tension), 150°F/85% RH to equilibrium (approximately 1.1% weight gain)
 0.610 ksiIPS Properties ( 45 tension), 150°F/85% RH to equilibrium (approximately 1.1% weight gain)
 0.720 ksiIPS Properties ( 45 tension)
 9.30 ksi
@Temperature 23.9 °C
90°
 353 ksi
@Temperature -59.4 °C
 364 ksi
@Temperature 23.9 °C
Elongation at Break 0.770 %
@Temperature 23.9 °C
90°
 1.46 %
@Temperature 23.9 °C
 1.52 %
@Temperature -59.4 °C
Tensile Modulus 1210 ksi
@Temperature 23.9 °C
90°
 22900 ksi
@Temperature -59.4 °C
 23500 ksi
@Temperature 23.9 °C
Flexural Strength 125 ksi
@Temperature 149 °C
0°, 1 week immersion in 160°F water
 162 ksi
@Temperature 121 °C
0°, 1 week immersion in 160°F water
 173 ksi
@Temperature 104 °C
0°, 1 week immersion in 160°F water
 246 ksi
@Temperature 104 °C
 256 ksi
@Temperature 23.9 °C
Flexural Modulus 1890 ksi
@Temperature 149 °C
0°, 1 week immersion in 160°F water
 2010 ksi
@Temperature 104 °C
0°, 1 week immersion in 160°F water
 2120 ksi
@Temperature 121 °C
0°, 1 week immersion in 160°F water
 2170 ksi
@Temperature 23.9 °C
 2220 ksi
@Temperature 104 °C
Compressive Strength 28.0 ksiAfter Impact, (25/50/25 orientation) 1500 in-lb/in. impact level
 37.0 ksi
@Temperature 104 °C
Open Hole, 25/50/25 orientation, wet
 46.7 ksi
@Temperature 23.9 °C
Open Hole, 25/50/25 orientation
 160 ksi
@Temperature 149 °C
0°, 1 week immersion in 160°F water
 195 ksi
@Temperature 121 °C
0°, 1 week immersion in 160°F water
 221 ksi
@Temperature 104 °C
0°, 1 week immersion in 160°F water
 244 ksi
@Temperature 23.9 °C
Compressive Modulus 21200 ksi
@Temperature 104 °C
0°, 1 week immersion in 160°F water
 21200 ksi
@Temperature 121 °C
0°, 1 week immersion in 160°F water
 21400 ksi
@Temperature 104 °C
 21700 ksi
@Temperature 149 °C
0°, 1 week immersion in 160°F water
 22300 ksi
@Temperature 23.9 °C
Shear Strength 9.00 ksi
@Temperature 149 °C
0°, Interlaminar, 1 week immersion in 160°F water
 11.4 ksi
@Temperature 121 °C
0°, Interlaminar, 1 week immersion in 160°F water
 12.9 ksi
@Temperature 104 °C
0°, Interlaminar, 1 week immersion in 160°F water
 13.6 ksi
@Temperature 104 °C
0°, Interlaminar
 18.5 ksi
@Temperature 23.9 °C
0°, Interlaminar
 
Processing PropertiesOriginal ValueComments
Shelf Life 0.300 Month
@Temperature 22.0 °C
 6.00 Month
@Temperature -18.0 °C
 
Descriptive Properties
G1 C1.8 in-lb/inInterlaminar Fracture Toughness, DCB
 3.3 in-lb/inInterlaminar Fracture Toughness, ENF

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PHEXCB9141 / 322297

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.