MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Arsenical Admiralty Copper, UNS C44300, H01 Temper tubing
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent cold workability for forming and bending.

Applications: condenser, evaporator and heat exchanger tubing, condenser tubing plates, distiller tubing, ferrules.

Test specimen: tubing - 25mm OD x 1.65mm wall thickness.

Key Words: Inhibited Admiralty Metal, Admiralty Brass, CDA 443, CZ111, ISO CuZn28Sn1As
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.53 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 434 MPa
Elongation at Break 45 %In 50 mm
Modulus of Elasticity 110 GPa
Poissons Ratio 0.38calculated
Fatigue Strength 115 - 125 MPa
@# of Cycles 1.00e+7
source does not state temper
Machinability 30 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 40.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000690 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 20.2 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.380 J/g-°C
Thermal Conductivity 110 W/m-K
@Temperature 20.0 °C
Melting Point 900 - 935 °C
Solidus 900 °C
Liquidus 935 °C
Annealing Point 800 - 1100 °F
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 425 - 600 °C
Hot-Working Temperature 650 - 800 °C
Recrystallization Temperature 300 °CFor 1 mm strip cold rolled hard(50% reduction), from 0.015 mm grain size
 
Component Elements PropertiesOriginal ValueComments
Arsenic, As 0.020 - 0.10 %
Copper, Cu 70 - 73 %
Iron, Fe <= 0.060 %
Lead, Pb <= 0.070 %
Tin, Sn 0.90 - 1.2 %
Zinc, Zn 28 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Special Metals MONEL® Alloy K-500
Overview of materials for Medium Carbon Steel
AISI Type 420F Stainless Steel, annealed bar
AISI 4140 Steel, oil quenched, 540°C (1000°F) temper, 25 mm (1 in.) round
ATI Allegheny Ludlum Martensitic Stainless Steel Type 410, Hardened + 649°C (1200°F) Temper

MC44300b4 / 11370

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.