MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Elektro-Isola Etronit IIQ R Phenolic, Paper Reinforcement, Yellow, Sheets
Categories: Polymer; Thermoset; Phenolic

Material Notes: Description: Mechanically a good Etronit type with electrical properties adequate for insulation in low-voltage applications.

Applications: Used in electrical appliances, bus-bar carriers, partition plates, and protection materials. With very low water absorption and good electrical properties.

Information provided by Elektro-Isola

Key Words: IEC/EN 60893-3-1 PF CP 203, NF C26 150 PP, BS 2572 P2, NEMA LI 1 XX
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.35 g/cc
@Temperature 23.0 °C
24h/23°C/50% RH; ISO 1183-A
Water Absorption 1.1 %ISO 62-1
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 110 MPa
@Thickness >=1.50 mm
24h/23°C/50% RH; ISO 527
Flexural Strength 160 MPa
@Thickness >=1.50 mm
24h/23°C/50% RH, Normal to laminate plane; ISO 178
Flexural Modulus 8.00 GPa
@Thickness >=1.50 mm
24h/23°C/50% RH, Normal to laminate plane; ISO 178
Compressive Strength 300 MPa
@Thickness >=5.00 mm
24h/23°C/50% RH, , Normal to laminate plane; ISO 604
Shear Strength 35.0 MPa
@Thickness >=5.00 mm
Parallel, 24h/23°C/50% RH; IEC 60893-2
Izod Impact, Notched (ISO) 3.30 kJ/m²
@Thickness >=5.00 mm
Parallel, 24h/23°C/50% RH; ISO 180/2A
 
Electrical PropertiesOriginal ValueComments
Insulation Resistance 1.00e+8 ohmafter immersion in water for 24 hr at 23°C; IEC 60167
Dielectric Constant 5.0
@Thickness <=3.00 mm,
Frequency 50 Hz
96h/105°C + 1h/23°C/20%RH; IEC 60250
Dielectric Strength 7.00 kV/mm
@Thickness 3.00 mm,
Temperature 90.0 °C
after 1 hour in oil, Normal to laminate plane; IEC 60243-1
 25.0 kV/in
@Thickness >=3.00 mm,
Temperature 90.0 °C
after 1 hour in oil, Parallel to laminate plane; IEC 60243-1
Dissipation Factor 0.040
@Thickness <=3.00 mm,
Frequency 50 Hz
96h/105°C + 1h/23°C/20%RH; IEC 60250
Comparative Tracking Index 100 V
@Thickness >=3.00 mm
24h/23°C/50% RH; IEC 60112
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 120 °C
@Thickness >=3.00 mm,
Time 7.20e+7 sec
IEC 60216
 
Descriptive Properties
ColorDark brown

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PELEKT029 / 126905

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.