MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Solvay FM® 385S Epoxy Film Adhesive
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Description: FM® 385 adhesive film was developed specifically for bonding composite and metallic structures for nacelle applications. It provides a unique combination of high Tg good toughness and very high flatwise tensile properties. FM 385 is designed for co-cure, co-bond or secondary bonding applications and is compatible with most 350°F (177°C) curing epoxy-based prepreg systems. It has excellent resistance to pre-bond and post-bond humidity and has a dry service temperature of 420°F (215°C). FM 385 adhesive film provides excellent handling properties (good tack and drape) and has a minimum shop life of 30 days at 75°F (24°C). FM 385 adhesive can be supplied as a supported (woven glass or mat carrier) or unsupported film at various weights and thicknesses. For co-cure or co-bond applications, adhesive film weight of 0.060 – 0.080 lb/ft2 with woven glass or a glass mat carrier is recommended. This adhesive film is suitable for bonding of monolithic or sandwich structures. Honeycomb sandwich panels manufactured using FM 385 adhesive film demonstrate excellent laminate quality (void content <1%) and very good filleting. FM 385 adhesive film can be cured at 350°F (177°C) in 90 minutes at 40 psi (0.28 MPa) or can be cured under vacuum-only pressure. Performance after vacuum-only cure is comparable to that after pressure cure. Cytec recommends using 250°F (121°C) curing BR® 6747-1 (chromated) or BR 6700 (non-chromated) water-based primers for metal bond applications using FM 385 adhesive film. For higher temperature applications or continuous service at 350°F (177°C), higher Tg BR 6800 non-chromated primer is recommended.

Features & Benefits:

  • Compatible with most 350°F (177°C) curing epoxy prepregs
  • Excellent fracture toughness (co-cure, co-bond or secondary bond)
  • Service temperature of 420°F (215°C) dry and 300°F (150°C) wet
  • Excellent resistance to both pre-bond and post-bond humidity
  • Good combination of peel and shear properties
  • Tg > 375°F (190°C)
  • Designed for bonding composite sandwich structures (good filleting properties)
  • Unsupported film designed for reticulation for acoustic structures
  • Highly flow controlled, good tack and handling properties
  • Shop life > 30 days at 75°F (24°C).
Applications:
  • Co-cure, co-bond and secondary bonding of metallic and composite structures for nacelle applications
  • Bonding of honeycomb sandwich structures

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.70 g/cc0.0614 lb/in³
Volatiles <= 1.0 %<= 1.0 %
Storage Temperature <= -18.0 °C<= -0.400 °F
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 5.86 MPa850 psiHoneycomb Flatwise after 250°F (121°C) wet 750 hours at 160°F (71°C)
 7.24 MPa1050 psiHoneycomb Flatwise after 75°F (24°C) wet 750 hours at 160°F (71°C)
 7.58 MPa1100 psiHoneycomb Flatwise after Salt spray, 75°F (24°C) 750 hours at 95°F (35°C); ASTM D1655
 8.529 MPa1237 psiHoneycomb Flatwise after Turbine Oil 168 hours at 75°F (24°C)
 8.632 MPa1252 psiHoneycomb Flatwise after Solvent (RIMS 1017 MEK/MIBK 168 hours at 75°F (24°C)
 8.729 MPa1266 psiHoneycomb Flatwise after Hydraulic Fluid 168 hours at 75°F (24°C)
 8.749 MPa1269 psiHoneycomb Flatwise after Deicing Fluid (AMS 1428) 168 hours at 75°F (24°C)
 9.067 MPa1315 psiHoneycomb Flatwise after Jet A. 75°F (24°C) 168 hours at 75°F (24°C)
 4.48 MPa
@Temperature 177 °C
650 psi
@Temperature 351 °F
Honeycomb Flatwise
 8.039 MPa
@Temperature 121 °C
1166 psi
@Temperature 250 °F
Honeycomb Flatwise
 9.65 MPa
@Temperature -59.0 °C
1400 psi
@Temperature -74.2 °F
Honeycomb Flatwise
 10.0 MPa
@Temperature 24.0 °C
1450 psi
@Temperature 75.2 °F
Honeycomb Flatwise
Shear Strength 27.6 MPa4000 psiLap after 250°F (121°C) wet 750 hours at 160°F (71°C)
 34.08 MPa4943 psiLap after Solvent (RIMS 1017 MEK/MIBK 168 hours at 75°F (24°C)
 35.0 MPa5080 psiLap after Salt spray, 75°F (24°C) 750 hours at 95°F (35°C)
 36.94 MPa5358 psiLap after Turbine Oil 168 hours at 75°F (24°C) per MIL-L-23699
 38.0 MPa5510 psiLap after Jet A. 75°F (24°C) 168 hours at 75°F (24°C) per ASTM D-1655
 38.6 MPa5600 psiLap after Hydraulic Fluid 168 hours at 75°F (24°C)
 40.3 MPa5840 psiLap after Deicing Fluid (AMS 1428) 168 hours at 75°F (24°C)
 22.50 MPa
@Temperature 177 °C
3264 psi
@Temperature 351 °F
Lap with Aluminum Substrates
 27.88 MPa
@Temperature 177 °C
4043 psi
@Temperature 351 °F
Double Lap with Aluminum Substrates
 31.0 MPa
@Temperature -59.0 °C
4500 psi
@Temperature -74.2 °F
Lap with Aluminum Substrates
 34.98 MPa
@Temperature 121 °C
5073 psi
@Temperature 250 °F
Double Lap with Aluminum Substrates, wet
 37.9 MPa
@Temperature 24.0 °C
5490 psi
@Temperature 75.2 °F
Lap with Aluminum Substrates
 40.50 MPa
@Temperature 121 °C
5874 psi
@Temperature 250 °F
Lap with Aluminum Substrates
 44.16 MPa
@Temperature 121 °C
6405 psi
@Temperature 250 °F
Double Lap with Aluminum Substrates
 49.98 MPa
@Temperature -59.0 °C
7249 psi
@Temperature -74.2 °F
Double Lap with Aluminum Substrates
 50.06 MPa
@Temperature 24.0 °C
7261 psi
@Temperature 75.2 °F
Double Lap with Aluminum Substrates
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 150 °C302 °Fwet
 215 °C419 °Fdry
 
Processing PropertiesMetricEnglishComments
Shelf Life 12.0 Month12.0 Month
 
Descriptive Properties
ColorDark Gray
Honeycomb Sandwich Peel32 in-lb/3in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Epoxy Adhesive
Trelleborg Emerson & Cuming Eccobond® 286 Two-Component General Purpose Epoxy Adhesive
Atom Adhesives AA-SUPERTHERM 195 Epoxy Adhesive
Atom Adhesives AA-DUCT N02 Epoxy Adhesive
Atom Adhesives AA-DUCT 902LP Epoxy Adhesive

PCYTED058 / 180360

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.