MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Ineos ABS Lustran® 266 ABS, Transparent Grade  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Transparent, Molded

Material Notes: Lustran® ABS 266 resin is a clear injection molding grade of ABS (acrylonitrile butadiene styrene). This transparent, general-purpose grade provides clarity and toughness with ease of processing. The resin is available in transparent tint, color code 000000. A tough, transparent grade of ABS, Lustran® ABS 266 resin is used in housings, toys, lawn and garden applications, and various consumer goods.

Lustran® is now a product of INEOS Styrolution. Information provided by the manufacturer.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.08 g/ccASTM-D792
Linear Mold Shrinkage 0.0040 - 0.0060 cm/cmASTM-D955
Melt Flow 5.0 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM-D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 108ASTM-D785
Tensile Strength at Break 30.0 MPaASTM-D638
Tensile Strength, Yield 37.0 MPaASTM-D638
Elongation at Break >= 48 %ASTM-D638
Elongation at Yield 4.0 %ASTM-D638
Tensile Modulus 2.00 GPaASTM-D638
Flexural Yield Strength 59.0 MPaASTM-D790
Flexural Modulus 1800 MPaASTM-D790
Izod Impact, Notched 176 J/m
@Thickness 3.20 mm
ASTM-D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear 121 µm/m-°CASTM-D696
Deflection Temperature at 0.46 MPa (66 psi) 87.0 °C
@Thickness 3.20 mm
Unannealed; ASTM-D648
 94.0 °C
@Thickness 12.7 mm
Unannealed; ASTM-D648
Deflection Temperature at 1.8 MPa (264 psi) 73.0 °C
@Thickness 3.20 mm
Unannealed; ASTM-D648
 82.0 °C
@Thickness 12.7 mm
Unannealed; ASTM-D648
UL RTI, Electrical 50.0 °C
@Thickness 1.50 mm
UL746B
UL RTI, Mechanical with Impact 50.0 °C
@Thickness 1.50 mm
UL746B
UL RTI, Mechanical without Impact 50.0 °C
@Thickness 1.50 mm
UL746B
Flammability, UL94 HB
@Thickness 1.50 mm
Clear Color
 HB
@Thickness 3.00 mm
Clear Color
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.52ASTM-D542
Haze 3.0 %
@Thickness 2.54 mm
ASTM-D1003
Transmission, Visible 86 %
@Thickness 2.54 mm
ASTM-D1003
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 195 - 220 °CInjection Molding
Middle Barrel Temperature 200 - 225 °CInjection Molding
Front Barrel Temperature 205 - 230 °CInjection Molding
Nozzle Temperature 205 - 230 °CInjection Molding
Melt Temperature 205 - 230 °CInjection Molding
Mold Temperature 45.0 - 65.0 °CInjection Molding
Drying Temperature 71.0 - 77.0 °C
@Time 14400 sec
 82.0 - 88.0 °C
@Time 7200 sec
Moisture Content <= 0.10 %
Dew Point <= -29.0 °Cinlet air
Injection Pressure 10000 - 16000 psiInjection Molding
Back Pressure 0.000 - 25.0 psiInjection Molding
Clamp Pressure 30.8 - 61.6 MPaInjection Molding
Cushion <= 0.250 inInjection Molding
 
Descriptive Properties
Hold Pressure50-75% of Injection Pressure, Injection Molding
Injection SpeedHighInjection Molding
Screw Compression Ratio2.5:1Injection Molding
Screw Length-to-Diameter Ratio>= 20:1Injection Molding
Screw SpeedModerate, Injection Molding
Shot Weight-to-Machine Capacity Ratio0.5-0.75Injection Molding

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chi Mei Polylac® PA-758 ABS - Transparent
INEOS Styrolution Terlux® 2802 Transparent MABS
INEOS Styrolution Terlux® HD 2802 MABS
INEOS Styrolution Terlux® 2802 TR Q434 Transparent MABS
LG Chemical TR557 MABS, High Transparency, High Impact

PINEA916 / 107187

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.