MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Magnesium M1A Sheet, Hard-Rolled
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes:

Key Words: UNS M15100; Mg
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.77 g/cc0.0639 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 5454500 kg load, 10 mm ball
Hardness, Knoop 6969Estimated from Brinell
Tensile Strength, Ultimate 240 MPa34800 psi
Tensile Strength, Yield 180 MPa
@Strain 0.2 %
26100 psi
@Strain 0.2 %
Elongation at Break 7.0 %7.0 %in 50 mm
Tensile Modulus 45.0 GPa6530 ksi
Compressive Yield Strength 125 MPa18100 psiat 0.2% offset
Ultimate Bearing Strength 395 MPa57300 psi
Bearing Yield Strength 270 MPa39200 psi
Poissons Ratio 0.350.35
Shear Modulus 17.0 GPa2470 ksi
Shear Strength 115 MPa16700 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000500 ohm-cm0.00000500 ohm-cm
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 370 J/g159 BTU/lbEstimated from trends in similar Mg alloys.
CTE, linear  26.0 µm/m-°C
@Temperature 0.000 - 100 °C
14.4 µin/in-°F
@Temperature 32.0 - 212 °F
 27.0 µm/m-°C
@Temperature 20.0 - 200 °C
15.0 µin/in-°F
@Temperature 68.0 - 392 °F
Estimated from similar Mg alloys
Specific Heat Capacity 1.00 J/g-°C0.239 BTU/lb-°FTypical Mg alloy value.
Melting Point 648 - 649 °C1200 - 1200 °F
Solidus 648 °C1200 °F
Liquidus 649 °C1200 °F
 
Component Elements PropertiesMetricEnglishComments
Calcium, Ca <= 0.30 %<= 0.30 %
Copper, Cu <= 0.050 %<= 0.050 %
Magnesium, Mg 99 %99 %As Remainder
Manganese, Mn >= 1.2 %>= 1.2 %
Nickel, Ni <= 0.010 %<= 0.010 %
Silicon, Si <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Magnesium EA65RS-T4, Extruded
Magnesium M1A-F Sheet, Annealed
Magnesium M1A-F, Extruded
Magnesium HK31A-O, Plate
Magnesium HK31A-T6, Sheet

MMM1A2 / 12457

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.