MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

ITW Devcon® DFense Blok™ Fast Cure (FC) Wear-Resistant Epoxy Compound
Categories: Polymer; Thermoset; Epoxy

Material Notes: Alumina ceramic bead-filled epoxy system with outstanding wear and abrasion resistance for severe service conditions. Fast cure allows for repaired processing equipment to be returned to service in as little as 2 hours. Uses: Repair scrubbers, ash handling systems, pipe elbows, screens, chutes, chippers, bins, hoppers, bunkers, separators and digester tables. Protect exhausters, launderers, housing fans, crushers, breakers, and conveyor screws. Features: Fast cure for minimal downtime, Superior wear and abrasion resistance, Able to withstand impact, Resistant to a wide range of chemicals, Non-sagging.

Information provided by ITW Performance Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.05 g/cc2.05 g/ccCured
Solids Content 100 %100 %Uncured
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8080
Flexural Strength 51.63 MPa7488 psiASTM D790
Compressive Strength 49.49 MPa7178 psiASTM D695
Adhesive Bond Strength 19.06 MPa2764 psiAdhesive Tensile Shear; ASTM D1002
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 4545ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 59.4 µm/m-°C33.0 µin/in-°FASTM D696
Maximum Service Temperature, Air 60.0 °C140 °FTemperature Resistance - Wet
 149 °C300 °FTemperature Resistance - Dry
Shrinkage 0.080 %0.080 %Linear During cure; ASTM D2566
 
Processing PropertiesMetricEnglishComments
Cure Time  120 - 180 min
@Temperature 24.0 °C
2.00 - 3.00 hour
@Temperature 75.2 °F
 600 min
@Temperature 24.0 °C
10.0 hour
@Temperature 75.2 °F
 10100 min
@Temperature 24.0 °C
168 hour
@Temperature 75.2 °F
As Tested
Pot Life 15.0 min
@Temperature 23.9 °C
15.0 min
@Temperature 75.0 °F
 
Descriptive Properties
Chemical/Solvent Resistance1,1,1-Trichloroethane: very good30 day immersion at 75°F. Sample cured 7 days at RT
 Ammonia: excellent30 day immersion at 75°F. Sample cured 7 days at RT
 Gasoline (Unleaded): fair30 day immersion at 75°F. Sample cured 7 days at RT
 Hydrochloric Acid 10%: very good30 day immersion at 75°F. Sample cured 7 days at RT
 Methanol: poor30 day immersion at 75°F. Sample cured 7 days at RT
 Methyl Ethyl Ketone: poor30 day immersion at 75°F. Sample cured 7 days at RT
 Sodium Hydroxide 50%: excellent30 day immersion at 75°F. Sample cured 7 days at RT
 Sulfuric Acid 10%: very good30 day immersion at 75°F. Sample cured 7 days at RT
 Trisodium Phosphate: very good30 day immersion at 75°F. Sample cured 7 days at RT
ColorGrayCured
Coverage53 sq. in/lbUncured at 1/4"
Mix Ratio by volume2:1
Mix Ratio by weight2:1
Recoat Time1 to 1.5 hrs
Specific Volume (in.³/lb)13.5Cured
ViscosityNon-sag putty Mixed

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PITWD9173 / 239683

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.