AISI 1547 Steel, annealed, cold drawn, 19-32 mm (0.75-1.25 in) round
Categories:
Metal
;
Ferrous Metal
;
Carbon Steel
;
AISI 1000 Series Steel
;
Medium Carbon Steel
Material Notes:
Suitable for forgings. Used in the production of rods and wires. This alloy was deleted as a SAE standard in 1977.
Key Words:
UNS G15470, ASTM A29, ASTM A510, ASTM A576, SAE J403, SAE J412, SAE J414
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
7.87
g/cc
0.284
lb/in³
Typical for steel
Mechanical Properties
Metric
English
Comments
Hardness, Brinell
187
187
Hardness, Knoop
209
209
Converted from Brinell
Hardness, Rockwell B
90
90
Converted from Brinell
Hardness, Rockwell C
10
10
Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
Hardness, Vickers
196
196
Converted from Brinell
Tensile Strength, Ultimate
655
MPa
95000
psi
Tensile Strength, Yield
585
MPa
84800
psi
Elongation at Break
10 %
10 %
Reduction of Area
35 %
35 %
Modulus of Elasticity
200
GPa
29000
ksi
Typical for steel
Bulk Modulus
160
GPa
23200
ksi
Typical for steel.
Poissons Ratio
0.29
0.29
Typical For Steel
Machinability
45 %
45 %
Based on 100% machinability for AISI 1212 steel.
Shear Modulus
80.0
GPa
11600
ksi
Typical for steel.
Electrical Properties
Metric
English
Comments
Electrical Resistivity
0.0000174
ohm-cm
0.0000174
ohm-cm
Typical steel
Thermal Properties
Metric
English
Comments
CTE, linear
11.5
µm/m-°C
@Temperature 20.0 °C
6.39
µin/in-°F
@Temperature 68.0 °F
Typical steel
12.2
µm/m-°C
@Temperature 0.000 - 300 °C
6.78
µin/in-°F
@Temperature 32.0 - 572 °F
Typical for steel
13.9
µm/m-°C
@Temperature 0.000 - 500 °C
7.72
µin/in-°F
@Temperature 32.0 - 932 °F
Typical for steel
Specific Heat Capacity
0.472
J/g-°C
0.113
BTU/lb-°F
Typical steel
Thermal Conductivity
51.9
W/m-K
360
BTU-in/hr-ft²-°F
Typical steel
Component Elements Properties
Metric
English
Comments
Carbon, C
0.43 - 0.51 %
0.43 - 0.51 %
Iron, Fe
97.75 - 98.22 %
97.75 - 98.22 %
As remainder
Manganese, Mn
1.35 - 1.65 %
1.35 - 1.65 %
Phosphorus, P
<= 0.040 %
<= 0.040 %
Sulfur, S
<= 0.050 %
<= 0.050 %
References
for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
AISI 1547 Steel, cold drawn, 19-32 mm (0.75-1.25 in) round
AISI 1552 Steel, Annealed and Cold Drawn Bar (UNS G15520)
AISI 1536 High Manganese Carbon Steel, Cold Drawn Bar
AISI 1541 Steel, Cold Drawn Bar (UNS G15410)
AISI 1541 Steel, Annealed and Cold Drawn Bar (UNS G15410)
M1547C / 7359
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.