MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Ovako S355J2 550 M (2723) Steel, +SH
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: General Information: S355J2 is a structural carbon-manganese steel suitable for e.g. mechanical engineering applications. Below, a number of closely related variants are presented.
520 M is M-steel variant of S355J2 is as rolled or normalize rolled contrition. 550M is drawn or peeled version of S355

Information provided by Ovako

Key Words: ASt 52, A52 FP, Q420q-D, 1501 Gr.224-460, A52 RBII
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell  <= 200
@Thickness 55.0 - 70.0 mm
<= 200
@Thickness 2.17 - 2.76 in
Round bar
 <= 200
@Thickness 70.0 - 120 mm
<= 200
@Thickness 2.76 - 4.72 in
Round bar
Tensile Strength  490 - 630 MPa
@Thickness 55.0 - 70.0 mm
71100 - 91400 psi
@Thickness 2.17 - 2.76 in
Round bar
 490 - 630 MPa
@Thickness 70.0 - 120 mm
71100 - 91400 psi
@Thickness 2.76 - 4.72 in
Round bar
Tensile Strength, Yield  >= 350 MPa
@Thickness 70.0 - 120 mm
>= 50800 psi
@Thickness 2.76 - 4.72 in
Round bar
 >= 380 MPa
@Thickness 55.0 - 70.0 mm
>= 55100 psi
@Thickness 2.17 - 2.76 in
Reh, Round bar
Elongation at Break  20 %
@Thickness 70.0 - 120 mm
20 %
@Thickness 2.76 - 4.72 in
Round bar
 22 %
@Thickness 55.0 - 70.0 mm
22 %
@Thickness 2.17 - 2.76 in
Round bar
Modulus of Elasticity 210 GPa30500 ksi
Poissons Ratio 0.300.30
Shear Modulus 80.0 GPa11600 ksi
Impact Test  27.0 J
@Thickness 55.0 - 70.0 mm,
Temperature -20.0 °C
19.9 ft-lb
@Thickness 2.17 - 2.76 in,
Temperature -4.00 °F
Round bar
 27.0 J
@Thickness 70.0 - 120 mm,
Temperature -20.0 °C
19.9 ft-lb
@Thickness 2.76 - 4.72 in,
Temperature -4.00 °F
Round bar
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
6.67 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
0.110 - 0.115 BTU/lb-°F
@Temperature 122 - 212 °F
Thermal Conductivity 40.0 - 45.0 W/m-K278 - 312 BTU-in/hr-ft²-°FAmbient temperature
Transformation Temperature 400 °C752 °FMS
 720 °C1330 °FAC1
 815 °C1500 °FAC3
 
Component Elements PropertiesMetricEnglishComments
Calcium, Ca <= 0.0020 %<= 0.0020 %
Carbon, C 0.050 - 0.20 %0.050 - 0.20 %
Copper, Cu <= 0.55 %<= 0.55 %
Iron, Fe 97.08 - 98.85 %97.08 - 98.85 %As Balance
Manganese, Mn 1.0 - 1.5 %1.0 - 1.5 %
Phosphorus, P <= 0.025 %<= 0.025 %
Silicon, Si 0.050 - 0.50 %0.050 - 0.50 %
Sulfur, S 0.020 - 0.040 %0.020 - 0.040 %
Vanadium, V 0.030 - 0.10 %0.030 - 0.10 %
 
Descriptive Properties
WeldabilityCEV 0.47max
 Pcm 0.3max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ovako S355J2 S355K2 Steel, +AR
Ovako S355J2 S355J2(M) Steel, +AR
Ovako S355J2 SB9813 Steel, +AR
Ovako S355J2 550 M (2723) Steel, +C
Ovako S355JR EN10025-2:2004 Steel

NOVAKO419 / 234718

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.