MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
NOVA Chemicals Sclair® 2607 HDPE Injection Molding Resin
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Injection Molded

Material Notes:

Butene Copolymer

Features:

  • Excellent stiffness
  • Good impact resistance
  • Low warpage

Additives:

  • Elevated levels of processing antioxidant

Applications:

  • Roll-out carts

United States: SCLAIR 2607 resin complies with the specifications contained in the U.S. Food and Drug Administration (FDA) regulation 21 CFR 177.1520 for olefin polymers, para. (c) 3.2a, and may thus be used in the United States as an article or component of an article intended for use in contact with food, without temperature or food-type restrictions, subject to technical suitability.

NOVA Chemicals polyethylene resins are biologically and chemically inert.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.947 g/ccASTM D792
Melt Flow 4.8 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 65ASTM D2240
Tensile Strength, Yield 22.0 MPaASTM D638
Elongation at Break 1000 %ASTM D638
Flexural Modulus 0.862 GPaASTM D790
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 122 °CASTM D1525
 
Processing PropertiesOriginal ValueComments
Melt Temperature 170 - 215 °C
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
NOVA Chemicals Sclair® 2709 HDPE Injection Molding Resin
NOVA Chemicals Sclair® 2710 HDPE Injection Molding Resin
NOVA Chemicals Sclair® 2712 HDPE Injection Molding Resin
Chevron Phillips Marlex® 9005 HDPE Injection Molding Resin
Dow DMDB-7950 NT 7 High Density Polyethylene Resin

PEHN1M / 35571

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.