MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Zotefoams ZOTEK® F 35 PVDF Foam
Categories: Polymer; Thermoplastic; Fluoropolymer; Polyvinylidene Fluoride (PVDF)

Material Notes: Zotek® F 35 is a closed cell foam made from Arkema Kynar® PVDF manufactured using nitrogen expansion technology to produce foams with exceptional cell size uniformity, low odor / high purity and outstanding physical attributes.

Information provided by Zotefoams

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.0330 g/cc0.00119 lb/in³ISO 845
Water Absorption 0.060 %0.060 %ISO 2896
 2.2 %2.2 %ASTM 1056
Cell Length 0.250 mm0.00984 in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 0.245 MPa35.5 psiISO 1798
Elongation at Break 90 %90 %
Compressive Yield Strength 0.0600 MPa
@Strain 25 %
8.70 psi
@Strain 25 %
ISO 7214
Tear Strength 0.700 kN/m3.99 pliISO 8067
Compression Set 20 %
@Time 79200 sec,
Strain 50 %
20 %
@Time 22.0 hour,
Strain 50 %
0.5 hr recovery; ISO 7214
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 0.0330 W/m-K0.229 BTU-in/hr-ft²-°Fmean temp of 0°C; ISO 8301
 0.0380 W/m-K0.264 BTU-in/hr-ft²-°Fmean temp of 40°C; DIN 52 612
 0.0460 W/m-K0.319 BTU-in/hr-ft²-°Fmean temp of 80°C; ASTM C 518
Maximum Service Temperature, Air 110 °C230 °F
Flammability, UL94 V-0V-0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Zotefoams ZOTEK® F 74 HT PVDF Foam
Zotefoams ZOTEK® F 40 HT PVDF Foam
Zotefoams ZOTEK® F 40 HT LS PVDF Foam
Zotefoams ZOTEK® N B50 High Performance Nylon Foam
Zotefoams ZOTEK® F OSU Rigid PVDF Foam

PZOTEF963 / 150719

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.