MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Evonik VESTAKEEP® 4500 G PEEK
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Unreinforced

Material Notes: VESTAKEEP® 4500 G is a high viscosity, fast cristallization, unreinforced polyether ether ketone for injection molding and extrusion. The semi-crystalline polymer features superior, thermal and chemical resistance. Parts made from VESTAKEEP® 4500 G are of low flammability. VESTAKEEP® 4500 G can be processed by common machines for thermoplastics. The manufacturer recommends a melt temperature between 370°C and 380°C during the injection molding process. The mold temperature should be within a range of 160°C to 200°C, preferably 180°C. VESTAKEEP® 4500 G is supplied as granules in 25kg boxes with moisture-proof polyethylene liners. Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C. Pigmentation may affect values
Dry properties listed below
Industrial Sector: Automotive and Mobility, Industry and Engineering, Energy, Oil and Gas
Processing: Injection molding, Extrusion
Delivery form: Pellets, Granules
Optics: Opaque
Resistance to: Heat (thermal stability), Fire / burn
Electrical: Insulating
Conformity: Food contact
Additives: Unfilled
Applications: General purpose
Processing: Profile extrusion, Sheet extrusion
Special Characteristics: Semi-crystalline, High viscosity
Color: Natural color
Chemical Resistance: General chemical resistance

Information provided by Evonik.

Vendors: Ensinger TECAPEEK™ shapes are manufactured exclusively with Victrex™ PEEK polymer. The Ensinger process and Victrex resins ensure reliability, consistency, dimensional stability, and high temperature mechanical performance.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.30 g/ccISO 1183
Viscosity 1120 cP
@Frequency 100 Hz,
Temperature 380 °C
Melt
Linear Mold Shrinkage, Flow 0.00900 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0120 cm/cmISO 294-4, 2577
Melt Flow 9.00 g/10 min
@Load 5.00 kg,
Temperature 380 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 86.0ISO 7619-1
Tensile Strength 96.0 MPaISO 527
Tensile Strength, Yield 96.0 MPaISO 527
Elongation at Break 30.0 %Nominal; ISO 527
 30.0 %ISO 527
Elongation at Yield 5.00 %ISO 527
Tensile Modulus 3800 MPaISO 527
Charpy Impact Unnotched NB
@Temperature 23.0 °C
ISO 179/1eU
 NB
@Temperature -40.0 °C
ISO 179/1eU
Charpy Impact, Notched 7.00 kJ/m²Type of failure: C; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+13 ohm-cm?V; IEC 62631-3-1
Dielectric Constant 3.30
@Thickness 2.00 mm,
Frequency 1.00e+6 Hz
IEC 62631-2-1
Dielectric Strength 24.3 kV/mm
@Thickness 1.00 mm
AC, S20/P25; IEC 60243-1
 29.2 kV/mm
@Thickness 1.00 mm
AC, P25/P25; IEC 60243-1
 29.4 kV/mm
@Thickness 0.990 mm
Short Time; ASTM D149
 35.2 kV/mm
@Thickness 1.00 mm
AC, S20/S20, t; IEC 60243-1
Dissipation Factor 0.00560
@Thickness 2.00 mm,
Frequency 1.00e+6 Hz
IEC 62631-2-1
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 69.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1/-2
CTE, linear, Transverse to Flow 64.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1/-2
Melting Point 340 °CISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 232 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 156 °CISO 75-1/-2
Glass Transition Temp, Tg 153 °CISO 11357
Flammability, UL94 V-0
@Thickness 3.20 mm
IEC 60695-11-10
Glow Wire Ignition Temperature 875 °C
@Thickness 2.00 mm
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 2.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Feed Temperature 60.0 °CInjection Molding
 60.0 °CPlastification
Zone 1 350 - 360 °CPlastification
Zone 2 350 - 360 °CPlastification
Zone 3 360 - 370 °CPlastification
Zone 4 360 - 370 °CPlastification
Zone 5 370 - 380 °CPlastification
Melt Temperature 380 °C
 380 °CInjection Molding; ISO 294
 380 - 390 °CPlastification
Mold Temperature 180 °CInjection Molding; ISO 294
 180 °C
Drying Temperature <= 150 °CPre-drying
 170 - 180 °CPre-drying, Pretreatment
Dry Time 4.00 - 6.00 hourPre-drying
 8.00 - 12.0 hourPre-drying, Pretreatment
Moisture Content <= 0.0200 %processing humidity
 
Descriptive Properties
ColorNatural Color

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PEVONIK7836 / 324968

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.