MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Aluminum 1100-H14
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 1000 Series Aluminum

Material Notes: This is a common commercial grade sold when 'aluminum' is specified. As with other unalloyed aluminum grades, it is used where the intrinsic formability and corrosion resistance of aluminum is needed while high strength is not. Example applications include chemical and food handling, sheet metal, hollowware, heat exchangers, and lighting.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
The aluminum content for unalloyed aluminum not made by a refining process is the difference between 100.00 percent and the sum of all other analyzed metallic elements present in amounts of 0.010 percent of more each, expressed to the second decimal before determining the sum. For alloys and unalloyed aluminum not made by a refining process, when the specified maximum limit is 0.XX, an observed value or a calculated value greater than 0.005 but less than 0.010% is rounded off and shown as " less than 0.01%".
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 1100-H14; UNS A91100; ISO Al99.0Cu; NF A45 (France); CSA 990C (Canada); AA1100-H14; Al1100-H14
Vendors: Visit metalmen for your commercially pure Aluminum 1100 needs. Stocking bar and plate for immediate delivery - unique in North America. Small quantities, cut to order. Contact us for sheet. coil and wire. Phone 1-800-767-9494..

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.71 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 32AA; Typical; 500 g load; 10 mm ball
Tensile Strength, Ultimate 18.0 ksiAA; Typical
 110 - 145 MPaWire and rod (rivet and cold heading grade)
 110 - 145 MPaSheet and plate
 14.0 MPa
@Temperature 371 °C
 20.0 MPa
@Temperature 316 °C
 28.0 MPa
@Temperature 260 °C
 69.0 MPa
@Temperature 204 °C
 97.0 MPa
@Temperature 149 °C
 110 MPa
@Temperature 100 °C
 125 MPa
@Temperature 24.0 °C
 130 MPa
@Temperature -28.0 °C
 140 MPa
@Temperature -80.0 °C
 205 MPa
@Temperature -195 °C
 >= 110 MPa
@Thickness <=9.50 mm
Wire, rod, and bar (rolled or cold finished)
 >= 110 MPa
@Thickness 0.356 - 12.7 mm
Drawn tube
Tensile Strength, Yield 17.0 ksiAA; Typical
 >= 95.0 MPaSheet and plate
 11.0 MPa
@Temperature 371 °C
 14.0 MPa
@Temperature 316 °C
 18.0 MPa
@Temperature 260 °C
 52.0 MPa
@Temperature 204 °C
 83.0 MPa
@Temperature 149 °C
 105 MPa
@Temperature 100 °C
 115 MPa
@Temperature -28.0 °C
 115 MPa
@Temperature 24.0 °C
 125 MPa
@Temperature -80.0 °C
 140 MPa
@Temperature -195 °C
Elongation at Break 1.0 - 10 %Sheet and plate
 20 %
@Temperature -28.0 °C
 20 %
@Temperature 24.0 °C
 20 %
@Temperature 100 °C
 23 %
@Temperature 149 °C
 24 %
@Temperature -80.0 °C
 26 %
@Temperature 204 °C
 45 %
@Temperature -195 °C
 75 %
@Temperature 260 °C
 80 %
@Temperature 316 °C
 85 %
@Temperature 371 °C
 9.0 %
@Thickness 1.59 mm
AA; Typical
 20 %
@Diameter 12.7 mm
AA; Typical
Modulus of Elasticity 10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Notched Tensile Strength 138 MPa2.5 cm width x 0.16 cm thick side-notched specimen, Kt = 17.
Ultimate Bearing Strength 200 MPaEdge distance/pin diameter = 2.0
Bearing Yield Strength 159 MPaEdge distance/pin diameter = 2.0
Poissons Ratio 0.33
Fatigue Strength 7000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Machinability 30 %0-100 Scale of Aluminum Alloys
Shear Modulus 26.0 GPa
Shear Strength 11.0 ksiAA; Typical
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000300 ohm-cm
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 390 J/g
CTE, linear 13.1 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 21.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
 24.5 µm/m-°C
@Temperature 20.0 - 200 °C
 25.5 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.904 J/g-°C
Thermal Conductivity 220 W/m-K
Melting Point 1190 - 1215 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 1190 °FAA; Typical
Liquidus 1215 °FAA; Typical
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.050Bare Metal
Reflection Coefficient, Visible (0-1) 0.86Tungsten Filament Source, Bare Metal
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 650 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al >= 99.00 %Specified
Beryllium, Be <= 0.0008 %welding electrode and filler wire only
Copper, Cu 0.05 - 0.20 %
Manganese, Mn <= 0.05 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Si+Fe <= 0.95 %
Zinc, Zn <= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 1100-O
Aluminum 1100-H12
Aluminum 1050-H14
Aluminum 1100-H16
Aluminum 1100-H18

MA1100H14 / 8747

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.