MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

INEOS Styrolution Zylar® 650 MBS
Categories: Polymer; Thermoplastic; Acrylic (PMMA)

Material Notes: Zylar® 650 is an impact modified styrene acrylic copolymer that provides a balance of clarity and toughness, with outstanding strength and rigidity. Zylar 650 also has superior processing characteristics for demanding injection molded applications.
  • Good balance of toughness, stiffness, and clarity
  • Low density
  • Ease of processing
  • Gamma & ETO sterilizable
  • Meets USP XXIII specifications for Class VI plastics

Information provided by Styrolution

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.04 g/cc0.0376 lb/in³ASTM D 792
Water Absorption at Saturation 0.10 %
@Temperature 23.0 °C
0.10 %
@Temperature 73.4 °F
ASTM D 570
Linear Mold Shrinkage 0.0020 - 0.0060 cm/cm0.0020 - 0.0060 in/inASTM D 955
Melt Flow 4.0 g/10 min
@Load 5.00 kg,
Temperature 200 °C
4.0 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 8484ASTM D 785
Tensile Strength, Yield 26.2 MPa3800 psiASTM D 638
Elongation at Break 40 %40 %ASTM D 638
Tensile Modulus 2.14 GPa310 ksiASTM D 638
Flexural Strength 48.3 MPa7000 psiASTM D 790
Flexural Modulus 1.93 GPa280 ksiASTM D 790
Izod Impact, Notched 1.60 J/cm3.00 ft-lb/inASTM D 256
Gardner Impact 16.9 J12.5 ft-lbASTM D 5420
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 249 °C480 °F
Vicat Softening Point 98.9 °C
@Load 1.02 kg
210 °F
@Load 2.25 lb
120°C/h; ASTM D 1525
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.57
@Wavelength 589.3 nm
1.57
@Wavelength 589.3 nm
Sodium D Line; ASTM D 542
Haze 2.0 %2.0 %ASTM D 1003
Transmission, Visible >= 90 %
@Wavelength 550 nm
>= 90 %
@Wavelength 550 nm
ASTM D 1003
 
Processing PropertiesMetricEnglishComments
Melt Temperature 204 - 238 °C400 - 460 °F
Mold Temperature 26.7 - 54.4 °C80.0 - 130 °F
Drying Temperature 65.6 °C
@Time 7200 sec
150 °F
@Time 2.00 hour
 
Compliance PropertiesMetricEnglishComments
USP Class VI YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
INEOS Styrolution Zylar® 960 MBS
Denka TP-803 Transparent Resin Polymer (MBS resin) Polymethacrylate Butadiene Styrene
Nitriflex Nitrimpact 1300 MBS Modifier
Ineos Nova Zylar® 631 Clear Impact Modified Acrylic Copolymer
INEOS Styrolution Clearblend 165 MBS

PBASF8032 / 159714

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.