MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Hytrel® 5526 TPC-ET
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester TPE

Material Notes: 55 Shore D High Performance High Flow Polyester Elastomer Developed for Injection Molding

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.19 g/ccISO 1183
Melt Density 1.04 g/cc
@Temperature 230 °C
Water Absorption 0.60 %
@Time 86400 sec
Immersion; Sim. to ISO 62
 0.60 %
@Thickness 2.00 mm
Sim. to ISO 62
Moisture Absorption 0.200 %
@Thickness 2.00 mm
Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.014 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.014 cm/cmISO 294-4, 2577
Melt Flow 17.5 g/10 min
@Load 2.16 kg,
Temperature 220 °C
cm³/10min Volumetric; ISO 1133
 18 g/10 min
@Load 2.16 kg,
Temperature 220 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 5115s; ISO 48-4
 <= 55ISO 48-4
Tensile Stress at Strain 6.90 MPa
@Strain 5.0 %
1BA specimen at 50mm/min; ISO 527-1/-2
 11.0 MPa
@Strain 10 %
ISO 527-1/-2
 14.0 MPa
@Strain 50 %
ISO 527-1/-2
Tensile Modulus 190 MPaISO 527-1/-2
Flexural Modulus 200 MPaISO 178
Poissons Ratio 0.48
Charpy Impact Unnotched NB
@Temperature -30.0 °C
ISO 179/1eU
 NB
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 30.0 kJ/m²
@Temperature -40.0 °C
ISO 179/1eA
 150 kJ/m²
@Temperature -30.0 °C
Partial Break; ISO 179/1eA
 NB
@Temperature 23.0 °C
ISO 179/1eA
Tensile Impact Strength 270 kJ/m²
@Temperature 23.0 °C
Notched; ISO 8256/1
Tensile Creep Modulus, 1 hour 170 MPa1h; ISO 899-1
Tensile Creep Modulus, 1000 hours 130 MPa1000h; ISO 899-1
Tear Strength 133 kN/mnormal; ISO 34-1
 133 kN/mparallel; ISO 34-1
Abrasion 120mm3; ISO 4649
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 4.00e+13 ohm-cmIEC 62631-3-1
Surface Resistance >= 1.00e+15 ohmIEC 62631-3-2
Dielectric Constant 4.6
@Frequency 1e+6 Hz
IEC 62631-2-1
 4.9
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 20.0 kV/mmIEC 60243-1
Dissipation Factor 0.0090
@Frequency 100 Hz
IEC 62631-2-1
 0.0375
@Frequency 1e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 600 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 200 µm/m-°CISO 11359-1/-2
 180 µm/m-°C
@Temperature -40.0 - 23.0 °C
ISO 11359-1/-2
CTE, linear, Transverse to Flow 200 µm/m-°CISO 11359-1/-2
 170 µm/m-°C
@Temperature -40.0 - 23.0 °C
ISO 11359-1/-2
Specific Heat Capacity 2.11 J/g-°C
@Temperature 230 °C
Melt
Thermal Conductivity 0.190 W/m-K
@Temperature 230 °C
Melt
Melting Point 203 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 65.0 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 45.0 °CISO 75-1/-2
Vicat Softening Point 75.0 °C50°C/h, 50N; ISO 306
 180 °C50°C/h 10N; ISO 306
Brittleness Temperature -98.0 °CISO 974
Glass Transition Temp, Tg -25.0 °C10°C/min; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 1.50 mm
IEC 60695-11-10
 HB
@Thickness 3.00 mm
IEC 60695-11-10
Flame Spread 28.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
Oxygen Index 21 %ISO 4589-1/-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 230 °COptimum, Injection
 220 - 250 °CRange, Injection
Mold Temperature 45.0 °COptimum, Injection
 45.0 - 55.0 °CInjection
Drying Temperature 100 °CInjection
Dry Time 2.00 - 3.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.080 %Injection
 
Descriptive Properties
Drying RecommendedyesInjection
Eff. thermal diffusivity (m²/s)9E-08
FMVSS ClassSE/BISO 3795 (FMVSS 302)
Fogging (mg)0.1G-value (condensate); ISO 6452
Odor Class5VDA 270
Part Marking Code>TPC-ET<ISO 11469
PolymerTPC
Resin IdentificationTPC-ETISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Hytrel® 4056 TPC-ET
Celanese Hytrel® 3078 TPC-ET
Celanese Hytrel® 6356 TPC-ET
Celanese Hytrel® 7246 TPC-ET
Celanese Hytrel® 4556 TPC-ET

PDSX5182 / 197822

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.