MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Titanium Beta III (Ti-11.5Mo-6Zr-4.5Sn; Grade 10), Solution Treated, Unaged
Categories: Metal; Nonferrous Metal; Titanium Alloy; Beta Titanium Alloy

Material Notes: Characteristics: Beta alloy, high strength, good hardenability, good resistance to stress corrosion, good cold-formability.

Applications: Aircraft fasteners and sheet metal parts, to a lesser extent - plate and forging applications.

5 other heat treatments of this alloy are in MatWeb.

Key Words: Ti-11.5Mo-6Zr-4.5Sn; UNS R58030; Beta 3
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 5.06 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 240
Tensile Strength, Ultimate 725 MPa
Tensile Strength, Yield 620 MPa
Elongation at Break 15 %
Reduction of Area 65 %
Modulus of Elasticity 79.0 GPa
Compressive Yield Strength 800 MPa
Poissons Ratio 0.36
Fracture Toughness 160 MPa-m½K(IC)
Shear Modulus 27.0 GPa
Shear Strength 590 MPaUltimate shear strength
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000156 ohm-cm
Magnetic Permeability 1.0
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.60 µm/m-°C
@Temperature 20.0 - 100 °C
 8.10 µm/m-°C
@Temperature 20.0 - 315 °C
average
 8.70 µm/m-°C
@Temperature 20.0 - 540 °C
average
Specific Heat Capacity 0.525 J/g-°CTypical value for titanium alloys.
Thermal Conductivity 6.28 W/m-K
Melting Point 1573 - 1690 °C
Solidus 1573 °C
Liquidus 1690 °C
Beta Transus 760 °CSlow transition kinetics
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.10 %
Hydrogen, H <= 0.020 %
Iron, Fe <= 0.35 %
Molybdenum, Mo 11.5 %
Nitrogen, N <= 0.050 %
Other, each <= 0.010 %
Other, total <= 0.040 %
Oxygen, O <= 0.18 %
Tin, Sn 4.5 %
Titanium, Ti 78 %
Zirconium, Zr 6.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Titanium Beta C (Ti-3Al-8V-6Cr-4Mo-4Zr) Solution Treated 815°C
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) Solution Treated 850°C (1560°F)
Titanium Beta C (Ti-3Al-8V-6Cr-4Mo-4Zr ST 815°C, Aged 565°C
Titanium Ti-11.5Mo-6Zr-4.5Sn, ST 720°C, Aged 495°C
Titanium Ti-15V-3Cr-3Al-3Sn Solution Treated

MTB030 / 14152

Metalmen Sales

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.