MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

SABIC NORYL™ Resin PX0844 Polyphenylene Ether + PS (PPE+PS) (Europe)
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene + Polyphenylene Ether, Unreinforced

Material Notes: NORYL™ PX0844 resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This grade exhibits very low moisture absorption, hydrolytic stability, dimensional stabilty, good foam adhesion, and property retention over a wide temperature range. NORYL PX0844 resin is inherently UL94 HB and is an excellent candidate for automotive interior applications such as instrument panels, audio components, speaker housings, and interior trim. *see NORYL PX0888 resin for higher heat resistance.

Features: Hydrolytic Stability,Low Creep Sensitivity

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.06 g/cc0.0383 lb/in³ISO 1183
Moisture Absorption 0.0300 %0.0300 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.14 %0.14 %ISO 62-1
Viscosity 9.0 cP
@Load 3.80 kg,
Temperature 280 °C
9.0 cP
@Load 8.38 lb,
Temperature 536 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inSABIC method
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 35.0 MPa5080 psi50 mm/min; ISO 527
Tensile Strength, Yield 45.0 MPa6530 psi50 mm/min; ISO 527
Elongation at Break 40 %40 %50 mm/min; ISO 527
Elongation at Yield 4.0 %4.0 %50 mm/min; ISO 527
Tensile Modulus 2.35 GPa341 ksi1 mm/min; ISO 527
Flexural Strength 65.0 MPa9430 psiyield, 2 mm/min; ISO 178
Flexural Modulus 2.20 GPa319 ksi2 mm/min; ISO 178
Izod Impact, Notched (ISO) 17.0 kJ/m²8.09 ft-lb/in²80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature -40.0 °C
2.38 ft-lb/in²
@Temperature -40.0 °F
80*10*4; ISO 180/1A
 10.0 kJ/m²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 80.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
44.4 µin/in-°F
@Temperature 73.4 - 176 °F
ISO 11359-2
CTE, linear, Transverse to Flow 90.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
50.0 µin/in-°F
@Temperature 73.4 - 176 °F
ISO 11359-2
Thermal Conductivity 0.230 W/m-K1.60 BTU-in/hr-ft²-°FISO 8302
Hot Ball Pressure Test 75.0 °C167 °FPASS; IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 122 °C252 °FEdgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi) 107 °C225 °FEdgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point 125 °C257 °FRate B/50; ISO 306
 128 °C262 °FRate B/120; ISO 306
 130 °C266 °FRate A/50; ISO 306
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 260 - 280 °C500 - 536 °F
Zone 2 260 - 280 °C500 - 536 °F
Zone 3 280 - 300 °C536 - 572 °F
Melt Temperature 280 - 300 °C536 - 572 °FInjection Molding
Mold Temperature 80.0 - 120 °C176 - 248 °F
Drying Temperature 100 - 120 °C212 - 248 °FInjection Molding
Dry Time 2.00 - 3.00 hour2.00 - 3.00 hourInjection Molding
Precipitation Temperature 60.0 - 80.0 °C140 - 176 °FHopper Temperature

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82431 / 290378

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.