Physical Properties | Metric | English | Comments |
---|
Density | 0.917 g/cc | 0.0331 lb/in³ |
Viscosity | 342 cP @Shear Rate 206 1/s, Temperature 200 °C | 342 cP @Shear Rate 206 1/s, Temperature 392 °F |
Melt Flow | 4.7 g/10 min @Load 2.16 kg, Temperature 230 °C | 4.7 g/10 min @Load 4.76 lb, Temperature 446 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore D | 44 @Time 15.0 sec | 44 @Time 0.00417 hour |
| 45 @Time 5.00 sec | 45 @Time 0.00139 hour |
| 47 @Time 1.00 sec | 47 @Time 0.000278 hour |
| 45 @Treatment Temp. 125 °C, Time 5.00 sec | 45 @Treatment Temp. 257 °F, Time 0.00139 hour |
| 47.2 @Treatment Temp. 110 °C, Time 15.0 sec | 47.2 @Treatment Temp. 230 °F, Time 0.00417 hour |
| 48.2 @Treatment Temp. 110 °C, Time 5.00 sec | 48.2 @Treatment Temp. 230 °F, Time 0.00139 hour |
| 49.2 @Treatment Temp. 125 °C, Time 15.0 sec | 49.2 @Treatment Temp. 257 °F, Time 0.00417 hour |
| 49.9 @Treatment Temp. 110 °C, Time 1.00 sec | 49.9 @Treatment Temp. 230 °F, Time 0.000278 hour |
| 51.5 @Treatment Temp. 125 °C, Time 1.00 sec | 51.5 @Treatment Temp. 257 °F, Time 0.000278 hour |
Tensile Strength at Break | 10.7 MPa | 1550 psi |
| 13.7 MPa | 1990 psi |
| 9.84 MPa @Treatment Temp. 110 °C, Time 3.629e+6 sec | 1430 psi @Treatment Temp. 230 °F, Time 1008 hour |
| 10.8 MPa @Treatment Temp. 125 °C, Time 605000 sec | 1570 psi @Treatment Temp. 257 °F, Time 168 hour |
| 15.4 MPa @Treatment Temp. 110 °C, Time 3.629e+6 sec | 2230 psi @Treatment Temp. 230 °F, Time 1008 hour |
| 17.7 MPa @Treatment Temp. 125 °C, Time 605000 sec | 2570 psi @Treatment Temp. 257 °F, Time 168 hour |
Tensile Stress at Strain | 8.69 MPa @Strain 100 % | 1260 psi @Strain 100 % |
| 12.5 MPa @Strain 100 % | 1820 psi @Strain 100 % |
| 9.82 MPa @Strain 100 %, Treatment Temp. 110 °C | 1420 psi @Strain 100 %, Treatment Temp. 230 °F |
| 10.2 MPa @Strain 100 %, Treatment Temp. 125 °C | 1470 psi @Strain 100 %, Treatment Temp. 257 °F |
| 15.4 MPa @Strain 100 %, Treatment Temp. 110 °C | 2240 psi @Strain 100 %, Treatment Temp. 230 °F |
| 17.7 MPa @Strain 100 %, Treatment Temp. 125 °C | 2570 psi @Strain 100 %, Treatment Temp. 257 °F |
Elongation at Break | 480 % | 480 % |
| 590 % | 590 % |
| 230 % @Treatment Temp. 125 °C, Time 605000 sec | 230 % @Treatment Temp. 257 °F, Time 168 hour |
| 245 % @Treatment Temp. 110 °C, Time 3.629e+6 sec | 245 % @Treatment Temp. 230 °F, Time 1008 hour |
| 301 % @Treatment Temp. 125 °C, Time 605000 sec | 301 % @Treatment Temp. 257 °F, Time 168 hour |
| 325 % @Treatment Temp. 110 °C, Time 3.629e+6 sec | 325 % @Treatment Temp. 230 °F, Time 1008 hour |
Tear Strength | 63.1 kN/m | 360 pli |
| 128 kN/m | 730 pli |
Compression Set | 39 % @Temperature 22.8 °C, Time 79200 sec | 39 % @Temperature 73.0 °F, Time 22.0 hour |
| 64 % @Temperature 70.0 °C, Time 79200 sec | 64 % @Temperature 158 °F, Time 22.0 hour |
| 78 % @Temperature 90.0 °C, Time 252000 sec | 78 % @Temperature 194 °F, Time 70.0 hour |
| 98 % @Temperature 125 °C, Time 252000 sec | 98 % @Temperature 257 °F, Time 70.0 hour |
|
Processing Properties | Metric | English | Comments |
---|
Processing Temperature | 190 - 230 °C | 374 - 446 °F |
Rear Barrel Temperature | 173 - 213 °C | 344 - 416 °F |
Middle Barrel Temperature | 179 - 219 °C | 354 - 426 °F |
Front Barrel Temperature | 184 - 224 °C | 364 - 436 °F |
Nozzle Temperature | 190 - 230 °C | 374 - 446 °F |
Zone 1 | 166 - 204 °C | 330 - 400 °F |
Zone 2 | 171 - 210 °C | 340 - 410 °F |
Zone 3 | 177 - 216 °C | 350 - 420 °F |
Zone 4 | 179 - 218 °C | 355 - 425 °F |
Zone 5 | 182 - 221 °C | 360 - 430 °F |
Die Temperature | 190 - 227 °C | 374 - 440 °F |
Mold Temperature | 35.0 - 60.0 °C | 95.0 - 140 °F |
Injection Pressure | 1.38 - 6.89 MPa | 200 - 1000 psi |
Back Pressure | 0.172 - 0.862 MPa | 25.0 - 125 psi |
Cushion | 0.381 - 2.54 cm | 0.150 - 1.00 in |
Screw Speed | 30 - 100 rpm | 30 - 100 rpm |
| 50 - 120 rpm | 50 - 120 rpm |
|
Descriptive Properties |
---|
Appearance | Opaque |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.