Physical Properties | Metric | English | Comments |
---|
Density | 7.90 g/cc | 0.285 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell B | <= 95 | <= 95 |
Tensile Strength, Ultimate | 580 - 780 MPa | 84100 - 113000 psi |
| >= 450 MPa @Temperature 500 °C | >= 65300 psi @Temperature 932 °F |
| >= 455 MPa @Temperature 450 °C | >= 66000 psi @Temperature 842 °F |
| >= 460 MPa @Temperature 400 °C | >= 66700 psi @Temperature 752 °F |
| >= 470 MPa @Temperature 350 °C | >= 68200 psi @Temperature 662 °F |
| >= 480 MPa @Temperature 300 °C | >= 69600 psi @Temperature 572 °F |
| >= 490 MPa @Temperature 250 °C | >= 71100 psi @Temperature 482 °F |
| >= 500 MPa @Temperature 200 °C | >= 72500 psi @Temperature 392 °F |
| >= 510 MPa @Temperature 150 °C | >= 74000 psi @Temperature 302 °F |
| >= 530 MPa @Temperature 100 °C | >= 76900 psi @Temperature 212 °F |
| >= 555 MPa @Temperature 50.0 °C | >= 80500 psi @Temperature 122 °F |
Tensile Strength, Yield | >= 270 MPa @Strain 0.2 % | >= 39200 psi @Strain 0.2 % |
| >= 300 MPa @Strain 1 % | >= 43500 psi @Strain 1 % |
| >= 140 MPa @Strain 0.2 %, Temperature 500 °C | >= 20300 psi @Strain 0.2 %, Temperature 932 °F |
| >= 145 MPa @Strain 0.2 %, Temperature 450 °C | >= 21000 psi @Strain 0.2 %, Temperature 842 °F |
| >= 155 MPa @Strain 0.2 %, Temperature 400 °C | >= 22500 psi @Strain 0.2 %, Temperature 752 °F |
| >= 165 MPa @Strain 0.2 %, Temperature 350 °C | >= 23900 psi @Strain 0.2 %, Temperature 662 °F |
| >= 170 MPa @Strain 1 %, Temperature 500 °C | >= 24700 psi @Strain 1 %, Temperature 932 °F |
| >= 175 MPa @Strain 0.2 %, Temperature 300 °C | >= 25400 psi @Strain 0.2 %, Temperature 572 °F |
| >= 175 MPa @Strain 1 %, Temperature 450 °C | >= 25400 psi @Strain 1 %, Temperature 842 °F |
| >= 185 MPa @Strain 1 %, Temperature 400 °C | >= 26800 psi @Strain 1 %, Temperature 752 °F |
| >= 190 MPa @Strain 0.2 %, Temperature 250 °C | >= 27600 psi @Strain 0.2 %, Temperature 482 °F |
| >= 195 MPa @Strain 1 %, Temperature 350 °C | >= 28300 psi @Strain 1 %, Temperature 662 °F |
| >= 200 MPa @Strain 0.2 %, Temperature 200 °C | >= 29000 psi @Strain 0.2 %, Temperature 392 °F |
| >= 215 MPa @Strain 0.2 %, Temperature 150 °C | >= 31200 psi @Strain 0.2 %, Temperature 302 °F |
| >= 215 MPa @Strain 1 %, Temperature 300 °C | >= 31200 psi @Strain 1 %, Temperature 572 °F |
| >= 215 MPa @Strain 1 %, Temperature 250 °C | >= 31200 psi @Strain 1 %, Temperature 482 °F |
| >= 230 MPa @Strain 1 %, Temperature 200 °C | >= 33400 psi @Strain 1 %, Temperature 392 °F |
| >= 230 MPa @Strain 0.2 %, Temperature 100 °C | >= 33400 psi @Strain 0.2 %, Temperature 212 °F |
| >= 245 MPa @Strain 1 %, Temperature 150 °C | >= 35500 psi @Strain 1 %, Temperature 302 °F |
| >= 250 MPa @Strain 0.2 %, Temperature 50.0 °C | >= 36300 psi @Strain 0.2 %, Temperature 122 °F |
| >= 260 MPa @Strain 1 %, Temperature 100 °C | >= 37700 psi @Strain 1 %, Temperature 212 °F |
| >= 285 MPa @Strain 1 %, Temperature 50.0 °C | >= 41300 psi @Strain 1 %, Temperature 122 °F |
Elongation at Break | >= 30 % | >= 30 % |
| >= 25 % @Thickness 50.8 mm | >= 25 % @Thickness 2.00 in |
Modulus of Elasticity | 195 GPa | 28300 ksi |
| 158 GPa @Temperature 500 °C | 22900 ksi @Temperature 932 °F |
| 166 GPa @Temperature 400 °C | 24100 ksi @Temperature 752 °F |
| 174 GPa @Temperature 300 °C | 25200 ksi @Temperature 572 °F |
| 182 GPa @Temperature 200 °C | 26400 ksi @Temperature 392 °F |
| 190 GPa @Temperature 100 °C | 27600 ksi @Temperature 212 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Magnetic Permeability | 1.003 | 1.003 |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 15.5 µm/m-°C @Temperature 30.0 - 100 °C | 8.61 µin/in-°F @Temperature 86.0 - 212 °F |
| 16.0 µm/m-°C @Temperature 30.0 - 200 °C | 8.89 µin/in-°F @Temperature 86.0 - 392 °F |
| 16.5 µm/m-°C @Temperature 30.0 - 300 °C | 9.17 µin/in-°F @Temperature 86.0 - 572 °F |
| 17.0 µm/m-°C @Temperature 30.0 - 400 °C | 9.44 µin/in-°F @Temperature 86.0 - 752 °F |
| 17.0 µm/m-°C @Temperature 30.0 - 600 °C | 9.44 µin/in-°F @Temperature 86.0 - 1110 °F |
| 17.0 µm/m-°C @Temperature 30.0 - 500 °C | 9.44 µin/in-°F @Temperature 86.0 - 932 °F |
| 17.5 µm/m-°C @Temperature 30.0 - 700 °C | 9.72 µin/in-°F @Temperature 86.0 - 1290 °F |
Specific Heat Capacity | 0.485 J/g-°C @Temperature 20.0 °C | 0.116 BTU/lb-°F @Temperature 68.0 °F |
| 0.505 J/g-°C @Temperature 100 °C | 0.121 BTU/lb-°F @Temperature 212 °F |
| 0.540 J/g-°C @Temperature 200 °C | 0.129 BTU/lb-°F @Temperature 392 °F |
| 0.565 J/g-°C @Temperature 300 °C | 0.135 BTU/lb-°F @Temperature 572 °F |
| 0.585 J/g-°C @Temperature 400 °C | 0.140 BTU/lb-°F @Temperature 752 °F |
| 0.605 J/g-°C @Temperature 500 °C | 0.145 BTU/lb-°F @Temperature 932 °F |
| 0.615 J/g-°C @Temperature 600 °C | 0.147 BTU/lb-°F @Temperature 1110 °F |
| 0.625 J/g-°C @Temperature 700 °C | 0.149 BTU/lb-°F @Temperature 1290 °F |
Thermal Conductivity | 13.0 W/m-K @Temperature 20.0 °C | 90.2 BTU-in/hr-ft²-°F @Temperature 68.0 °F |
| 15.0 W/m-K @Temperature 100 °C | 104 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 17.0 W/m-K @Temperature 200 °C | 118 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 19.0 W/m-K @Temperature 300 °C | 132 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 21.0 W/m-K @Temperature 400 °C | 146 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 23.0 W/m-K @Temperature 500 °C | 160 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 25.0 W/m-K @Temperature 600 °C | 174 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 26.0 W/m-K @Temperature 700 °C | 180 BTU-in/hr-ft²-°F @Temperature 1290 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | <= 0.020 % | <= 0.020 % |
Chromium, Cr | 25 % | 25 % |
Iron, Fe | 48.6 % | 48.6 % |
Manganese, Mn | 1.7 % | 1.7 % |
Molybdenum, Mo | 2.1 % | 2.1 % |
Nickel, Ni | 22 % | 22 % |
Nitrogen, N | 0.12 % | 0.12 % |
Phosphorus, P | <= 0.015 % | <= 0.015 % |
Silicon, Si | <= 0.40 % | <= 0.40 % |
Sulfur, S | <= 0.010 % | <= 0.010 % |