MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Eastman Tritan™ VX401 Copolyester
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: Product Description: Eastman Tritan™ VX401 is an amorphous copolyester with excellent clarity and impact resistance. The outstanding chemical resistance, hydrolytic stability, and ease of processing make Tritan™ VX401 an ideal candidate for a broad spectrum of optical applications such sunglass lenses, optical glass lenses and safety eyewear.

Application/Uses:

  • Light transmitting media
  • Machine guards
  • Optical glass lenses
  • Safety eyewear
  • Sunglass lenses
Key Attributes:
  • Ease of processing
  • Excellent clarity
  • Excellent hydrolytic stability
  • Outstanding impact resistance
  • Quick cycle times
  • Superior chemical resistance

Information provided by Eastman

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.17 g/cc0.0423 lb/in³ASTM D792
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 115115ASTM D785
Tensile Strength at Break 53.0 MPa7690 psiASTM D638
Tensile Strength, Yield 44.0 MPa6380 psiASTM D638
Elongation at Break 140 %140 %ASTM D638
Elongation at Yield 7.0 %7.0 %ASTM D638
Tensile Modulus 1.585 GPa229.9 ksiASTM D638
Flexural Yield Strength 66.0 MPa9570 psiASTM D790
Flexural Modulus 1.585 GPa229.9 ksiASTM D790
Izod Impact, Notched  1.26 J/cm
@Temperature -40.0 °C
2.36 ft-lb/in
@Temperature -40.0 °F
ASTM D256
 6.50 J/cm
@Temperature 23.0 °C
12.2 ft-lb/in
@Temperature 73.4 °F
ASTM D256
Izod Impact, Unnotched  NB
@Temperature -40.0 °C
NB
@Temperature -40.0 °F
ASTM D4812
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ASTM D4812
Puncture Energy  59.0 J
@Temperature 23.0 °C
43.5 ft-lb
@Temperature 73.4 °F
Energy @ Max. Load; ASTM D3763
 63.0 J
@Temperature -40.0 °C
46.5 ft-lb
@Temperature -40.0 °F
Energy @ Max. Load; ASTM D3763
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 109 °C228 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 92.0 °C198 °FASTM D648
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.561.56ASTM D1648
Abbe Number 30.8130.81ASTM C1648
Haze <= 0.40 %<= 0.40 %ASTM D1003
Transmission, Visible 92 %92 %Total; ASTM D1003
 
Processing PropertiesMetricEnglishComments
Melt Temperature 260 - 282 °C500 - 540 °F
Mold Temperature 38.0 - 66.0 °C100 - 151 °F
Drying Temperature 88.0 °C190 °F
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Eastman Tritan™ MX731 Medical Grade Copolyester
Eastman Tritan™ MXF121 Medical Grade Copolyester
EMS-Grivory Grilamid® TR 30 nat PA*
EMS-Grivory Grilamid® TR 90 UV PAMACM12
Eastman Tritan™ TXF1021 Copolyester

PEATM5202 / 222396

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.