MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Röhm Acrylite Plus® NTA-3 NTA Compound  (discontinued **)
Categories: Polymer; Thermoplastic; Acrylic (PMMA); Acrylic, Impact Modified, Molded

Material Notes: High heat deflection temperature and impact strength on same level as standard ACRYLITE polymers, optimized for thermal/hemidity cycling test.

Information Provided by Evonik CYRO. The former Evonik Methacrylates business has been sold to Röhm (Roehm) GmbH.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.19 g/cc1.19 g/ccISO 1183
Water Absorption <= 0.30 %<= 0.30 %ASTM D570
Linear Mold Shrinkage 0.0070 - 0.0080 cm/cm0.0070 - 0.0080 in/inISO 294
Melt Flow 3.1 g/10 min
@Load 3.80 kg,
Temperature 230 °C
3.1 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 70.3 MPa10200 psiISO 527
Elongation at Break 3.4 %3.4 %ISO 527
Elongation at Yield 3.4 %3.4 %ISO 527
Tensile Modulus 3.10 GPa450 ksiISO 527
Flexural Strength 80.7 MPa11700 psiISO 178
Flexural Modulus 3.10 GPa450 ksiISO 178
Izod Impact, Unnotched (ISO) 1.50 kJ/m²
@Diameter 4.00 mm
0.714 ft-lb/in²
@Diameter 0.157 in
bar; ISO 180
 
Thermal PropertiesMetricEnglishComments
CTE, linear 73.8 µm/m-°C
@Temperature 0.000 - 100 °C
41.0 µin/in-°F
@Temperature 32.0 - 212 °F
ISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 111 °C232 °Fannealed; ISO 75
Vicat Softening Point 115 °C239 °FISO 306
 
Optical PropertiesMetricEnglishComments
Transmission, Visible 0.0 %0.0 %Opaque; ASTM D1003
 
Processing PropertiesMetricEnglishComments
Middle Barrel Temperature 221 - 260 °C430 - 500 °FCylinder Temp
Melt Temperature 221 - 260 °C430 - 500 °F
Mold Temperature 48.9 - 85.0 °C120 - 185 °F
Drying Temperature 100 °C212 °F
Dry Time 2 - 3 hour2 - 3 hour

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Röhm Acrylite® 8N Acrylic Polymer
Röhm Acrylite® 8N df 20 Acrylic Polymer
Röhm Acrylite Plus® zdf Impact Acrylic Polymer
Röhm Acrylite Plus® zk3HR Impact Acrylic Polymer
Röhm Acrylite Plus® zk4BR Impact Acrylic Polymer

PCYR00049 / 89053

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.