MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Haynes HR-160® alloy plate, aged 8000 hours at 649°C (1200°F)
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Outstanding resistance to various forms of high-temperature corrosion attack, excellent resistance to sulfidation and chloride attack in both reducing and oxidizing atmospheres. Excellent forming and welding characteristics. Applications include a variety of fabricated components in municipal, industrial, hazardous, and nuclear waste heat recovery systems. Also suitable for utility boilers, sulfur plants, high-temperature furnaces, kilns, calciners, resource recovery units, cement kilns, pulp and paper recovery boilers, coal gasification systems, and fluidized-bed-combustion systems.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS N12160, ASTM B435, ASTM B366, DIN No.2.4880
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.08 g/ccat RT
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 843 MPa
Tensile Strength, Yield 353 MPa
@Strain 0.2 %
Elongation at Break 34 %in 50.8 mm
Reduction of Area 28 %
Modulus of Elasticity 211 GPaRT
 137 GPa
@Temperature 980 °C
 145 GPa
@Temperature 925 °C
 150 GPa
@Temperature 870 °C
 154 GPa
@Temperature 815 °C
 158 GPa
@Temperature 760 °C
 163 GPa
@Temperature 705 °C
 168 GPa
@Temperature 650 °C
 173 GPa
@Temperature 595 °C
 177 GPa
@Temperature 540 °C
 180 GPa
@Temperature 480 °C
 183 GPa
@Temperature 425 °C
 187 GPa
@Temperature 370 °C
 192 GPa
@Temperature 315 °C
 197 GPa
@Temperature 260 °C
 201 GPa
@Temperature 205 °C
 204 GPa
@Temperature 150 °C
 208 GPa
@Temperature 90.0 °C
 210 GPa
@Temperature 40.0 °C
Charpy Impact 42.0 Jaged 8000 hours at 650°C (1200°F)
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0001112 ohm-cmRT
 0.0001231 ohm-cm
@Temperature 700 °C
 0.0001238 ohm-cm
@Temperature 800 °C
 0.0001245 ohm-cm
@Temperature 900 °C
 0.0001252 ohm-cm
@Temperature 1000 °C
 0.0001259 ohm-cm
@Temperature 1100 °C
 0.0001267 ohm-cm
@Temperature 1200 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.0 µm/m-°C
@Temperature 25.0 - 95.0 °C
 13.7 µm/m-°C
@Temperature 25.0 - 205 °C
 14.0 µm/m-°C
@Temperature 25.0 - 315 °C
 14.4 µm/m-°C
@Temperature 25.0 - 425 °C
 14.9 µm/m-°C
@Temperature 25.0 - 540 °C
 15.5 µm/m-°C
@Temperature 25.0 - 600 °C
 15.7 µm/m-°C
@Temperature 25.0 - 700 °C
 16.6 µm/m-°C
@Temperature 25.0 - 800 °C
 17.1 µm/m-°C
@Temperature 25.0 - 900 °C
Specific Heat Capacity 0.462 J/g-°CRT
 0.653 J/g-°C
@Temperature 700 °C
 0.672 J/g-°C
@Temperature 800 °C
 0.689 J/g-°C
@Temperature 900 °C
 0.719 J/g-°C
@Temperature 1100 °C
 0.732 J/g-°C
@Temperature 1200 °C
 0.784 J/g-°C
@Temperature 1000 °C
Thermal Conductivity 10.9 W/m-KRT
 21.8 W/m-K
@Temperature 600 °C
 24.7 W/m-K
@Temperature 700 °C
 26.1 W/m-K
@Temperature 800 °C
 26.9 W/m-K
@Temperature 900 °C
 28.7 W/m-K
@Temperature 1000 °C
 31.1 W/m-K
@Temperature 1100 °C
 32.9 W/m-K
@Temperature 1200 °C
Melting Point 1293 - 1370 °C
Solidus 1293 °C
Liquidus 1370 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.050 %
Chromium, Cr 28 %
Cobalt, Co 30 %
Iron, Fe <= 3.5 %
Manganese, Mn 0.50 %
Molybdenum, Mo <= 1.0 %
Nickel, Ni 37 %
Niobium, Nb (Columbium, Cb) <= 1.0 %
Silicon, Si 2.75 %
Titanium, Ti 0.50 %
Tungsten, W <= 1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
446 Stainless Steel, Annealed Bar
446 Stainless Steel, Annealed and Cold Drawn Bar
Haynes Hastelloy® C-4 alloy, sheet, aged 100 hours at 899°C
Haynes Hastelloy® C-4 alloy, plate, heat treated at 1066°C, rapid quenched
Haynes Hastelloy® C-4 alloy, all-weld metal, as welded, GTAW

NH16AZ / 16348

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.