MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Evonik VESTAMID® eCO E40 CC50 Nylon 12, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12)

Material Notes: VESTAMID® eCO E40 CC50 is a PA 12 elastomer consisting of PA 12 segments and softening segments. The material is free of volatile or migrating plasticizer. The VESTAMID® E represents thermoplastic elastomers generically characterized as polyether block copolyamides (PEBA) consisting of PA 12 and polyether segments. VESTAMID® eCO E40 CC50 is especially developed for sport shoe soles. It has good impact strength at low temperatures. eCO stands for Evoniks aim to reduce CO2 trough use of renewable or circular feedstocks via mass-balance approach. VESTAMID® eCO E40 CC50 is supplied as spherical pellets in moisture-proof packaging, ready for processing. The process temperatures should be within a range of 170°C – 210°C. Pigmentation may affect values. Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.
Industrial Sector: Sustainable, Industry and Engineering, Sports and Lifestyle
Sustainability: RFP (reducted foot print), eCO
Processing: Injection molding, Extrusion
Delivery form: Pellets, Granules
Optics: Translucent
Resistance to: Heat (thermal stability), UV / light / weathering
Additives: Unfilled
Processing: Profile extrusion
Special Characteristics: Light-stabilized, U.V. stabilized, High heat resistant
Color: Natural color
Additives: Plasticizer, Light stabilizer, Heat stabilizer

Information provided by Evonik.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.01 g/cc0.0365 lb/in³ISO 1183
Water Absorption 1.00 %1.00 %Sim to ISO 62
Moisture Absorption 0.400 %0.400 %Sim to ISO 62
Viscosity Number 190 cm³/g1.90 dl/gISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.00500 cm/cm0.00500 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0110 cm/cm0.0110 in/inISO 294-4, 2577
Melt Flow 40.0 g/10 min
@Load 2.16 kg,
Temperature 240 °C
40.0 g/10 min
@Load 4.76 lb,
Temperature 464 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Puncture Resistance  880 N
@Temperature 23.0 °C
198 lb (f)
@Temperature 73.4 °F
ISO 6603-2
 1740 N
@Temperature -30.0 °C
391 lb (f)
@Temperature -22.0 °F
ISO 6603-2
Hardness, Shore D 40.0
@Time 3.00 sec
40.0
@Time 0.000833 hour
ISO 7619-1
Tensile Strength 17.0 MPa2470 psiISO 527
Tensile Stress 22.4 MPa3250 psiTPE; ISO 527
 4.30 MPa
@Strain 5.00 %
624 psi
@Strain 5.00 %
ISO 527
 6.40 MPa
@Strain 10.0 %
928 psi
@Strain 10.0 %
ISO 527
 8.50 MPa
@Strain 20.0 %
1230 psi
@Strain 20.0 %
ISO 527
 9.00 MPa
@Strain 50.0 %
1310 psi
@Strain 50.0 %
ISO 527
 10.0 MPa
@Strain 50.0 %
1450 psi
@Strain 50.0 %
ISO 527
 11.6 MPa
@Strain 100 %
1680 psi
@Strain 100 %
ISO 527
 20.9 MPa
@Strain 300 %
3030 psi
@Strain 300 %
ISO 527
Elongation at Break 200 %200 %nom. strain at br., etB; ISO 527
 333 %333 %TPE; ISO 527
Tensile Modulus 0.0870 GPa12.6 ksiISO 527
Flexural Modulus 0.0900 GPa13.1 ksiISO 178
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eA
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eA
Tensile Impact Strength 160 kJ/m²76.1 ft-lb/in²notched, atN; ISO 8256/1
Puncture Energy  14.0 J
@Temperature 23.0 °C
10.3 ft-lb
@Temperature 73.4 °F
ISO 6603-2
 25.0 J
@Temperature -30.0 °C
18.4 ft-lb
@Temperature -22.0 °F
ISO 6603-2
Taber Abrasion, mg/1000 Cycles <= 15.0<= 15.0S33, 2x 500g; DIN 53754
Compression Set  32.0 %
@Temperature 23.0 °C,
Time 86400 sec
32.0 %
@Temperature 73.4 °F,
Time 24.0 hour
 47.0 %
@Temperature 70.0 °C,
Time 86400 sec
47.0 %
@Temperature 158 °F,
Time 24.0 hour
ISO 815
 84.0 %
@Temperature 100 °C,
Time 86400 sec
84.0 %
@Temperature 212 °F,
Time 24.0 hour
ISO 815
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 2.00e+9 ohm-cm2.00e+9 ohm-cmIEC 62631-3-1
Dielectric Constant  4.90
@Frequency 1.00e+6 Hz
4.90
@Frequency 1.00e+6 Hz
IEC 62631-2-1
 7.50
@Frequency 100 Hz
7.50
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 35.0 kV/mm889 kV/inAC, S20/S20, t.; IEC 60243-1
Dissipation Factor  0.0700
@Frequency 100 Hz
0.0700
@Frequency 100 Hz
IEC 62631-2-1
 0.120
@Frequency 1.00e+6 Hz
0.120
@Frequency 1.00e+6 Hz
IEC 62631-2-1
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 240 µm/m-°C
@Temperature 25.0 - 55.0 °C
133 µin/in-°F
@Temperature 77.0 - 131 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 210 µm/m-°C
@Temperature 25.0 - 55.0 °C
117 µin/in-°F
@Temperature 77.0 - 131 °F
ISO 11359-1/-2
Melting Point 150 °C302 °FISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 55.0 °C131 °FISO 75-1/-2
Vicat Softening Point  60.0 °C
@Load 5.10 kg
140 °F
@Load 11.2 lb
50 K/h; ISO 306
 125 °C
@Load 1.02 kg
257 °F
@Load 2.25 lb
50 K/h; ISO 306
Glass Transition Temp, Tg -60.0 °C-76.0 °FISO 11357-1/-2
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
IEC 60695-11-10
 
Processing PropertiesMetricEnglishComments
Melt Temperature >= 180 °C>= 356 °FInjection Molding; ISO 294
 200 °C392 °F
Mold Temperature 35.0 °C95.0 °F
 35.0 °C95.0 °FInjection Molding; ISO 294
Injection Velocity 200 mm/sec7.87 in/secInjection Molding; ISO 294
Injection Pressure 70.0 MPa10200 psiInjection Molding; ISO 294
 
Descriptive Properties
Blue water consumption68.1 kgISO 14040, 14044
ColorBlack
Global Warming Potential2.5 kg CO2 eq./kgsavings incl. bio. C. as compared to classical production, ISO 14040, 14044
 4.2 kg CO2 eq./kgincl. bio. C incl. LUC, ISO 14040, 14044
 4.3 kg CO2 eq./kgexcl. bio. C incl. LUC, ISO 14040, 14044
Land use (ReCiPe 2016)0.6 Annual crop eq. yISO 14040, 14044

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEVONIK7899 / 325031

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.