MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Pressure Seal 8746 Fluorinated Hydrocarbon
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 8746 is a 70 durometer black colored Fluorinated Hydrocarbon elastomer, it is formulated with DuPont Viton®. It exhibits good resistance to heat, compression set and petroleum based oils.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 HK 815 A1-10 B37 B38 EF31 EO78 Z1; 4 HK 815 A1-11 B38 EF31 EO78 Z1; 6 HK 815 A1-10 A1-11 B31 B38 EF31 EO88 Z1
Z1 = Shore A Durometer 75 ± 5

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.85 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 75
 67
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 68
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 71
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
 73
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
 73
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 74
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 75
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 75
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 75
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 75
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
Tensile Strength 1878 psi
 1425.4 psi
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 1500.5 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 1538 psi
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
 1556.9 psi
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 1750.3 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 1842.3 psi
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
 1846.1 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 1900.5 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
Elongation, Ultimate 230 %
 210 %
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
 210 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 220.1 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 230 %
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 230 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 234.6 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 239.9 %
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 239.9 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 239.9 %
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
100% Modulus 611 psi
Tear Strength 137 pliDie B
 137 pliDie C
Compression Set 7.9 %
@Treatment Temp. 175 °C,
Time 79200 sec
Plied
 9.8 %
@Treatment Temp. 200 °C,
Time 79200 sec
Plied
 10 %
@Treatment Temp. 23.0 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -6.00 °F
Shrinkage 0.10 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 0.20 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 1.7 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #3
 1.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel B
 2.5 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, Distilled water aged
 4.1 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 8.8 %
@Treatment Temp. 200 °C,
Time 252000 sec
Volume, Service Fluid 100
 15.6 %
@Treatment Temp. 200 °C,
Time 252000 sec
Volume, Stauffer Blend 7700
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL103 / 318313

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.