MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Mocom (ALBIS) ALCOM® PP 620/9 MRX80 PP
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer

Material Notes: Base Polymer: Polypropylene Random Copolymer

Filler/Additive System: special filler

Special Features: High density

Market Segment: Furniture, Building and Construction, Sport and Leisure

Application Area: Injection molded parts

Typical Application: Fixing elements

Information provided by Albis Plastics

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.60 g/cc0.0939 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0090 - 0.011 cm/cm
@Time 86400 sec
0.0090 - 0.011 in/in
@Time 24.0 hour
ISO 294-4
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm
@Time 86400 sec
0.0050 - 0.0070 in/in
@Time 24.0 hour
ISO 294-4
Melt Flow 3.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
3.0 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 10.0 MPa1450 psiISO 527
Elongation at Break 1.6 %1.6 %ISO 527
Elongation at Yield 0.50 %0.50 %ISO 527
Tensile Modulus 3.20 GPa464 ksiISO 527
Flexural Strength 20.0 MPa2900 psiISO 178
Flexural Modulus 4.50 GPa653 ksiISO 178
Charpy Impact Unnotched 1.00 J/cm²4.76 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 0.350 J/cm²1.67 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 75.0 °C167 °FISO 75-1/-2
Vicat Softening Point 88.0 °C190 °FB50; ISO 306
 
Processing PropertiesMetricEnglishComments
Melt Temperature 200 - 270 °C392 - 518 °FInjection molding
Mold Temperature 20.0 - 90.0 °C68.0 - 194 °FInjection molding
Drying Temperature  60.0 - 90.0 °C
@Time 7200 - 14400 sec
140 - 194 °F
@Time 2.00 - 4.00 hour
in a dry air (desiccant) dryer
 60.0 - 90.0 °C
@Time 7200 - 14400 sec
140 - 194 °F
@Time 2.00 - 4.00 hour
in an circulating dryer
 
Descriptive Properties
Base PolymerPolypropylene Random Copolymer

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman PP 1500X-01 Polypropylene High Impact Copolymer Polypropylene
Aclo Accucomp Polypropylene CPO425BAV Automotive Approved Copolymer Expandable Grade
A. Schulman PP 2407 Polypropylene Impact Resistant Copolymer Polypropylene
Amco PRIMATOP PP CO 350-40 Polypropylene Copolymer
Amco PRIMATOP PP CO 350-20 Impact Polypropylene Copolymer

PALBIS8578 / 242637

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.