MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

ExxonMobil Bicor™ 26MB777 OPP Film  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polypropylene (PP); Polypropylene, Film Grade

Material Notes: Product Description: A high gas barrier, biaxially oriented transparent polypropylene film, coated on one side PVdC, one side acrylic. This film provides outstanding performance on all packaging machines.

Availability: Africa & Middle East, Asia Pacific and Europe

Key Features:

  • Excellent moisture, oxygen and aroma barriers
  • Excellent seal strength and hot tack
  • Excellent retention of PVdC seals in humid conditions
  • Outstanding optical properties
  • Ideal support for water based ink printing on acrylic side
  • Water base coatings
Features:
  • Acrylic Coated
  • Flavor & Aroma Barrier
  • Gas Barrier
  • Humidity Resistant
  • In Lamination Lap Sealable
  • Moisture Barrier
  • Oxygen Barrier
  • PVdC Coated
Applications:
  • Bakery
  • Biscuits/Cookie/Crackers
  • Box Overwrap
  • Confectionery, Chocolate
  • Confectionery, Gum
  • Confectionery, Sugar
  • Crisps and Snacks
  • Dairy Products
  • Dry Foods and Beverage Powders
  • Health and Beauty Care
  • Household and Detergents
  • Ice Cream
  • Pet Food
Uses:
  • Box Overwrap Flexible Packaging
  • HFFS Flexible Packaging
  • Pre-made Bags – Flexible Packaging
  • VFFS Flexible Packaging
Processing Method: Cold Seal Adhesive, Inner Web Adhesive Lamination, Outer Web Adhesive Lamination, Solvent Flexographic Printing, Solvent Rotogravure Printing and Surface Print Unsupported

Information provided by ExxonMobil

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Water Vapor Transmission  0.900 g/m²/day
@Temperature 23.0 °C
0.0580 g/100 in²/day
@Temperature 73.4 °F
85% RH; ExxonMobil Method
 4.19 g/m²/day
@Temperature 38.0 °C
0.270 g/100 in²/day
@Temperature 100 °F
90% RH; ExxonMobil Method
Oxygen Transmission Rate  20.0 cc/m²/day
@Temperature 23.0 °C
1.29 cc/100 in²/day
@Temperature 73.4 °F
Wet, 75% RH; ExxonMobil Method
 20.2 cc/m²/day
@Temperature 23.0 °C
1.30 cc/100 in²/day
@Temperature 73.4 °F
0% RH; ExxonMobil Method
Thickness 25.4 microns1.00 milExxonMobil Method
Coating Weight 24.6 g/m²15.4 lb/reamExxonMobil Method
 
Mechanical PropertiesMetricEnglishComments
Film Elongation at Break, MD 175 %175 %7.9 in/min, 4.9 in Jaw Separation; ExxonMobil Method
Film Elongation at Break, TD 60 %60 %7.9 in/min, 4.9 in Jaw Separation; ExxonMobil Method
Modulus of Elasticity 2.00 GPa290 ksiMD; ExxonMobil Method
 3.80 GPa551 ksiTD; ExxonMobil Method
Coefficient of Friction 0.250.25Acrylic; ExxonMobil Method
 0.350.35PVdC; ExxonMobil Method
Seal Strength  510 g/25 mm
@Pressure 0.276 MPa,
Temperature 140 °C
510 g/in
@Pressure 40.0 psi,
Temperature 284 °F
PVdC, 0.2 sec; ExxonMobil Method
 510 g/25 mm
@Pressure 0.276 MPa,
Temperature 130 °C
510 g/in
@Pressure 40.0 psi,
Temperature 266 °F
Acrylic, 0.2 sec; ExxonMobil Method
Film Tensile Strength at Break, MD 160 MPa23200 psi7.9 in/min, 4.9 in Jaw Separation; ExxonMobil Method
Film Tensile Strength at Break, TD 290 MPa42100 psi7.9 in/min, 4.9 in Jaw Separation; ExxonMobil Method
 
Thermal PropertiesMetricEnglishComments
Shrinkage, MD 6.0 %
@Temperature 135 °C,
Time 432 sec
6.0 %
@Temperature 275 °F,
Time 0.120 hour
ExxonMobil Method
Shrinkage, TD 5.5 %
@Temperature 135 °C,
Time 432 sec
5.5 %
@Temperature 275 °F,
Time 0.120 hour
ExxonMobil Method
 
Optical PropertiesMetricEnglishComments
Haze 1.6 %1.6 %ExxonMobil Method
Gloss 98 %98 %45°; ExxonMobil Method
 
Descriptive Properties
Carbon Dioxide Transmission Rate5.16 cc/100 in2/ 24 hr75% RH, ASTM D1434
Heat Seal Range54°FPVdC, 36.3 psi, 0.2 sec
 90°FAcrylic, 36.3 psi, 0.2 sec
Nitrogen Transmission Rate0.645 cc/100 in2/ 24 hr75% RH, ASTM D1434
Yield28100 in2/lb

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEX99481 / 175717

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.