MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Chosun Refractories SR Blast Furnace Runner Refractory
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes:

Information provided by Chosun Refractories via Korea Institute of Ceramic Engineering and Technology (KICET).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density  2.66 g/cc
@Temperature 1500 °C,
Time 10800 sec
0.0961 lb/in³
@Temperature 2730 °F,
Time 3.00 hour
 2.68 g/cc
@Temperature 110 °C,
Time 86400 sec
0.0968 lb/in³
@Temperature 230 °F,
Time 24.0 hour
 
Mechanical PropertiesMetricEnglishComments
Modulus of Rupture  0.0047088 GPa
@Temperature 110 °C,
Time 86400 sec
0.68296 ksi
@Temperature 230 °F,
Time 24.0 hour
 0.01393 GPa
@Temperature 1500 °C,
Time 10800 sec
2.020 ksi
@Temperature 2730 °F,
Time 3.00 hour
Compressive Strength  0.1268 MPa
@Treatment Temp. 1500 °C,
Time 10800 sec
18.39 psi
@Treatment Temp. 2730 °F,
Time 3.00 hour
Cold Crushing Strength
 36.2 MPa
@Treatment Temp. 110 °C,
Time 86400 sec
5250 psi
@Treatment Temp. 230 °F,
Time 24.0 hour
Cold Crushing Strength
 
Component Elements PropertiesMetricEnglishComments
Al2O3 67 %67 %
 
Descriptive Properties
Chemical Analysis(%) SiC+C17
Installation MethodCasing Vibration
Main ApplicationsSlag Iron runner
Material Required for Estimating (kg/m3)2,850
Water Required for Casting(%)6.5

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

CCHOS273 / 124217

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.