MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
Teknor Apex Monprene® MP-2090C Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Monprene MP-2090C is a high performance thermoplastic elastomer designed for a variety of consumer product applications requiring soft, rubber-like feel. Monprene MP-2090C is a low hardness, low density, RoHS compliant grade that is suitable for injection molding and extrusion.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Contact Clarity; Good Colorability; Good Flexibility; Good Melt Strength; Good Mold Release; Good Moldability; Good Processability; Good Processing Stability; High Elongation; Low Flow; Low Density; Low Specific Gravity; Lubricated; Low Hardness; Slip; Without Fillers

Uses: Consumer Applications; Gaskets; Handles; Rubber Replacement; Sporting Goods; Tubing; Writing Instruments

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Extrusion; Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.900 g/ccASTM D792
Melt Flow 5.0 g/10 min
@Load 5.00 kg,
Temperature 200 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 42
@Time 5.00 sec
Injection Molded; ASTM D2240
 44
@Time 1.00 sec
Injection Molded; ASTM D2240
Tensile Strength at Break 890 psi20 in/min, Flow; ASTM D412
 1260 psi20 in/min, Across Flow; ASTM D412
Tensile Stress at Strain 161 psi
@Strain 100 %
20 in/min, Across Flow; ASTM D412
 238 psi
@Strain 100 %
20 in/min, Flow; ASTM D412
 336 psi
@Strain 300 %
20 in/min, Across Flow; ASTM D412
 466 psi
@Strain 300 %
20 in/min, Flow; ASTM D412
Elongation at Break 640 %20 in/min, Flow; ASTM D412
 780 %20 in/min, Across Flow; ASTM D412
Tear Strength 159 pli20 in/min, Flow; ASTM D624
 204 pli20 in/min, Across Flow; ASTM D624
Compression Set 17 %
@Temperature 22.8 °C,
Time 79200 sec
ASTM D395B
 
Processing PropertiesOriginal ValueComments
Processing Temperature 420 - 460 °FMelt, Injection
Rear Barrel Temperature 420 - 460 °FInjection
Middle Barrel Temperature 420 - 460 °FInjection
Front Barrel Temperature 420 - 460 °FInjection
Nozzle Temperature 420 - 460 °FInjection
Zone 1 400 - 440 °FExtrusion
Zone 2 400 - 440 °FExtrusion
Zone 3 400 - 440 °FExtrusion
Zone 4 400 - 440 °FExtrusion
Zone 5 400 - 440 °FExtrusion
Die Temperature 400 - 440 °FExtrusion
Mold Temperature 60.0 - 90.0 °FInjection
Injection Pressure 200 - 800 psiInjection
Back Pressure 25.0 - 100 psiInjection
Cushion 0.150 - 1.00 inInjection
Screw Speed 30 - 100 rpmExtrusion
 50 - 100 rpmInjection
 
Descriptive Properties
AppearanceColors Available
 Natural Color
 Translucent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNQ0876 / 237367

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.