Physical Properties | Metric | English | Comments |
---|
Density | 7.90 g/cc | 0.285 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength, Ultimate | 1400 - 1600 MPa @Thickness 3.00 - 3.50 mm | 203000 - 232000 psi @Thickness 0.118 - 0.138 in |
| 1550 - 1750 MPa @Thickness 2.00 - 2.50 mm | 225000 - 254000 psi @Thickness 0.0787 - 0.0984 in |
| 1550 - 1750 MPa @Thickness 2.50 - 3.00 mm | 225000 - 254000 psi @Thickness 0.0984 - 0.118 in |
| 1700 - 1800 MPa @Thickness 1.25 - 1.50 mm | 247000 - 261000 psi @Thickness 0.0492 - 0.0591 in |
| 1700 - 1800 MPa @Thickness 1.50 - 2.00 mm | 247000 - 261000 psi @Thickness 0.0591 - 0.0787 in |
| 1800 - 1900 MPa @Thickness 0.800 - 1.00 mm | 261000 - 276000 psi @Thickness 0.0315 - 0.0394 in |
| 1800 - 1900 MPa @Thickness 25.4 - 31.8 mm | 261000 - 276000 psi @Thickness 1.00 - 1.25 in |
| 1900 - 2100 MPa @Thickness 0.650 - 0.800 mm | 276000 - 305000 psi @Thickness 0.0256 - 0.0315 in |
| 1900 - 2100 MPa @Thickness 0.500 - 0.650 mm | 276000 - 305000 psi @Thickness 0.0197 - 0.0256 in |
| 2000 - 2200 MPa @Thickness 0.300 - 0.400 mm | 290000 - 319000 psi @Thickness 0.0118 - 0.0157 in |
| 2000 - 2200 MPa @Thickness 0.400 - 0.500 mm | 290000 - 319000 psi @Thickness 0.0157 - 0.0197 in |
| 2050 - 2250 MPa @Thickness 0.200 - 0.300 mm | 297000 - 326000 psi @Thickness 0.00787 - 0.0118 in |
| 1400 - 1600 MPa @Diameter 3.50 - 4.00 mm | 203000 - 232000 psi @Diameter 0.138 - 0.157 in |
| 2100 - 2300 MPa @Diameter 0.150 - 0.200 mm | 305000 - 334000 psi @Diameter 0.00591 - 0.00787 in |
Tensile Strength, Yield | 1200 MPa @Thickness 3.00 - 3.50 mm | 174000 psi @Thickness 0.118 - 0.138 in |
| 1320 MPa @Thickness 2.00 - 2.50 mm | 191000 psi @Thickness 0.0787 - 0.0984 in |
| 1320 MPa @Thickness 2.50 - 3.00 mm | 191000 psi @Thickness 0.0984 - 0.118 in |
| 1440 MPa @Thickness 1.25 - 1.50 mm | 209000 psi @Thickness 0.0492 - 0.0591 in |
| 1440 MPa @Thickness 1.50 - 2.00 mm | 209000 psi @Thickness 0.0591 - 0.0787 in |
| 1520 MPa @Thickness 0.800 - 1.00 mm | 220000 psi @Thickness 0.0315 - 0.0394 in |
| 1520 MPa @Thickness 1.00 - 1.25 mm | 220000 psi @Thickness 0.0394 - 0.0492 in |
| 1600 MPa @Thickness 0.650 - 0.800 mm | 232000 psi @Thickness 0.0256 - 0.0315 in |
| 1600 MPa @Thickness 0.500 - 0.650 mm | 232000 psi @Thickness 0.0197 - 0.0256 in |
| 1680 MPa @Thickness 0.300 - 0.400 mm | 244000 psi @Thickness 0.0118 - 0.0157 in |
| 1680 MPa @Thickness 0.400 - 0.500 mm | 244000 psi @Thickness 0.0157 - 0.0197 in |
| 1720 MPa @Thickness 0.200 - 0.300 mm | 249000 psi @Thickness 0.00787 - 0.0118 in |
| 1200 MPa @Diameter 3.00 - 4.00 mm, Strain 0.2 % | 174000 psi @Diameter 0.118 - 0.157 in, Strain 0.2 % |
| 1760 MPa @Diameter 0.150 - 0.200 mm, Strain 0.2 % | 255000 psi @Diameter 0.00591 - 0.00787 in, Strain 0.2 % |
Modulus of Elasticity | 180 GPa | 26100 ksi |
| 190 GPa | 27600 ksi |
Poissons Ratio | 0.30 | 0.30 |
Shear Modulus | 69.0 GPa | 10000 ksi |
| 73.0 GPa | 10600 ksi |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0000700 ohm-cm @Temperature 20.0 °C | 0.0000700 ohm-cm @Temperature 68.0 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 16.5 µm/m-°C @Temperature 20.0 - 100 °C | 9.17 µin/in-°F @Temperature 68.0 - 212 °F |
| 17.0 µm/m-°C @Temperature 20.0 - 200 °C | 9.44 µin/in-°F @Temperature 68.0 - 392 °F |
| 18.0 µm/m-°C @Temperature 20.0 - 300 °C | 10.0 µin/in-°F @Temperature 68.0 - 572 °F |
Maximum Service Temperature, Air | 250 °C | 482 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | 0.11 % | 0.11 % |
Chromium, Cr | 18.5 % | 18.5 % |
Iron, Fe | 67.3 % | 67.3 % |
Manganese, Mn | 6.0 % | 6.0 % |
Nickel, Ni | 7.0 % | 7.0 % |
Nitrogen, N | 0.25 % | 0.25 % |
Phosphorus, P | <= 0.030 % | <= 0.030 % |
Silicon, Si | 0.80 % | 0.80 % |
Sulfur, S | <= 0.015 % | <= 0.015 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.