MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Latrobe LSS™ H10 Hot Work Tool Steel (ASTM H10)
Categories: Metal; Ferrous Metal; Alloy Steel; Chrome-moly Steel; Tool Steel; Hot Work Steel

Material Notes: TLS H10 hot work tool steel is a chromium-molybdenum hot work steel that exhibits excellent resistance to softening at elevated temperature. This grade is very resistant to thermal fatigue cracking (heat checking), and can be water cooled in service. TLS H10 is recommended for difficult hot work tooling applications such as hot punches, die casting dies, forging dies, hot shear blades, hot gripper dies, and extrusion tooling.

Information Provided by Timken Latrobe Steel.

Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 7.78 g/cc7.78 g/cc
Density 7.78 g/cc0.281 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 4141Air Cooled from 1024°C and Double Tempered; 649°C Temper Temperature
 5858Air Cooled from 1024°C and Double Tempered; 149°C Temper Temperature
Modulus of Elasticity 207 GPa30000 ksi
Machinability 90 - 95 %90 - 95 %1% Carbon Steel
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.3 µm/m-°C
@Temperature 21.0 - 204 °C
6.28 µin/in-°F
@Temperature 69.8 - 399 °F
 13.5 µm/m-°C
@Temperature 21.0 - 538 °C
7.50 µin/in-°F
@Temperature 69.8 - 1000 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 830 °C1530 °FCritical Temperaure Ac1
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.42 %0.42 %
Chromium, Cr 3.15 %3.15 %
Iron, Fe 92.38 %92.38 %
Manganese, Mn 0.55 %0.55 %
Molybdenum, Mo 2.15 %2.15 %
Silicon, Si 1.0 %1.0 %
Vanadium, V 0.35 %0.35 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Crucible Steel PDCQ Premium Quality High Toughness H13 Steel
Latrobe LSS™ H11 Hot Work Tool Steel (ASTM H11)
Crucible Steel CHRO-MOW® Tool Steel, AISI H12
Crucible Steel HALCOMB® 218 Tool Steel, AISI H11
Latrobe LSS™ H12 Hot Work Tool Steel (ASTM H12)

NTIMK079 / 19426

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.