MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Crastin® LW9020FR NC010 PBT+ASA-GF20FR(17)  (discontinued **)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); PBT + ASA Blend, Glass Fiber Reinforced

Material Notes: 20% Glass Reinforced, Flame Retardant, Polybutylene Terephthalate Blend with Low Warpage Characteristics

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.52 g/ccISO 1183
Melt Density 1.36 g/cc
@Temperature >=225 °C
Water Absorption 0.78 %
@Thickness 2.00 mm
Sim. to ISO 62
Moisture Absorption 0.230 %
@Thickness 2.00 mm
Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0040 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0080 cm/cmISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 110 MPaISO 527-1/-2
Elongation at Break 2.0 %ISO 527-1/-2
Tensile Modulus 8500 MPaISO 527-1/-2
Flexural Strength 155 MPaISO 178
Poissons Ratio 0.34ISO 527-1/-2
Izod Impact, Notched (ISO) 33.0 kJ/m²
@Temperature 23.0 °C
ISO 180/1U
 33.0 kJ/m²
@Temperature -30.0 °C
ISO 180/1U
Izod Impact, Unnotched (ISO) 6.00 kJ/m²
@Temperature 23.0 °C
ISO 180/1A
 6.00 kJ/m²
@Temperature -30.0 °C
ISO 180/1A
Charpy Impact Unnotched 35.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
 40.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 6.50 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 7.00 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
Tensile Creep Modulus, 1 hour 7500 MPaISO 899-1
Tensile Creep Modulus, 1000 hours 6000 MPaISO 899-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 62631-3-1
Surface Resistance 1.00e+14 ohmIEC 62631-3-2
Dielectric Constant 3.5
@Frequency 1e+6 Hz
IEC 62631-2-1
 3.7
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 29.0 kV/mmIEC 60243-1
 20.0 kV/mm
@Thickness 2.00 mm
20s; IEC 60243-1
 20.0 kV/mm
@Thickness 2.00 mm
Short Time; IEC 60243-1
 29.0 kV/mm
@Thickness 1.00 mm
Short Time; IEC 60243-1
Dissipation Factor 0.00175
@Frequency 100 Hz
IEC 62631-2-1
 0.015
@Frequency 1e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 300 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 30.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 100 µm/m-°CISO 11359-1/-2
Specific Heat Capacity 1.90 J/g-°C
@Temperature >=225 °C
Melt
Thermal Conductivity 0.250 W/m-K
@Temperature >=225 °C
Melt
Melting Point 225 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 215 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 175 °CISO 75-1/-2
Flammability, UL94 V-0
@Thickness 1.50 mm
IEC 60695-11-10
 V-0
@Thickness 3.00 mm
IEC 60695-11-10
Oxygen Index 27 %ISO 4589-1/-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 240 - 260 °CInjection
 250 °CInjection Optimum
Mold Temperature 30.0 - 130 °CInjection
 80.0 °CInjection Optimum
Ejection Temperature 170 °CInjection
Drying Temperature 120 °CInjection
Dry Time 2.00 - 4.00 hourDehumidified Dryer; Injection
Moisture Content 0.040 %Injection
Hold Pressure 60.0 MPaInjection
 
Descriptive Properties
AdditivesRelease agent
Back pressureAs low as possibleInjection
Delivery formPellets
Drying RecommendedyesInjection
FMVSS ClassDNIISO 3795 (FMVSS 302)
Hold pressure time (s/mm)3Injection
Part Marking CodePBT+ASA-GF20FR(17)ISO 11469
ProcessingInjection Molding
Regional AvailabilityAsia Pacific
 Europe
 Global
 Near East/Africa
 North America
 South and Central America
Resin IdentificationPBT+ASA-GF20FR(17)ISO 1043

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Crastin® SK643FR BK851 PBT-GF20FR(17)
Celanese Crastin® LW9020FR BK851 PBT+ASA-GF20FR(17)
A. Schulman SCHULADUR® A GF10 10% Glass Fiber Reinforced PBT
Overview of materials for Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled
Overview of materials for Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled

PZDSX5028 / 197668

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.