Physical Properties | Metric | English | Comments |
---|
Density | 0.924 g/cc | 0.0334 lb/in³ |
Melt Flow | 0.88 g/10 min @Load 2.16 kg, Temperature 190 °C | 0.88 g/10 min @Load 4.76 lb, Temperature 374 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Film Tensile Strength at Yield, MD | 11.8 MPa @Thickness 0.0508 mm | 1710 psi @Thickness 0.00200 in |
| 11.9 MPa @Thickness 0.0254 mm | 1730 psi @Thickness 0.00100 in |
Film Tensile Strength at Yield, TD | 12.2 MPa @Thickness 0.0508 mm | 1770 psi @Thickness 0.00200 in |
| 12.3 MPa @Thickness 0.0254 mm | 1780 psi @Thickness 0.00100 in |
Film Elongation at Break, MD | 270 % @Thickness 0.0254 mm | 270 % @Thickness 0.00100 in |
| 370 % @Thickness 0.0508 mm | 370 % @Thickness 0.00200 in |
Film Elongation at Break, TD | 540 % @Thickness 0.0254 mm | 540 % @Thickness 0.00100 in |
| 560 % @Thickness 0.0508 mm | 560 % @Thickness 0.00200 in |
2% Secant Modulus | 0.197 GPa @Thickness 0.0254 mm | 28.6 ksi @Thickness 0.00100 in |
| 0.201 GPa @Thickness 0.0508 mm | 29.2 ksi @Thickness 0.00200 in |
| 0.225 GPa @Thickness 0.0254 mm | 32.6 ksi @Thickness 0.00100 in |
| 0.227 GPa @Thickness 0.0508 mm | 32.9 ksi @Thickness 0.00200 in |
Elmendorf Tear Strength MD | 190 g @Thickness 0.0254 mm | 190 g @Thickness 0.00100 in |
| 400 g @Thickness 0.0508 mm | 400 g @Thickness 0.00200 in |
Elmendorf Tear Strength TD | 180 g @Thickness 0.0254 mm | 180 g @Thickness 0.00100 in |
| 450 g @Thickness 0.0508 mm | 450 g @Thickness 0.00200 in |
Dart Drop Test | 78.0 g @Thickness 0.0254 mm | 0.172 lb @Thickness 0.00100 in |
| 120 g @Thickness 0.0508 mm | 0.265 lb @Thickness 0.00200 in |
Film Tensile Strength at Break, MD | 21.6 MPa @Thickness 0.0508 mm | 3130 psi @Thickness 0.00200 in |
| 25.4 MPa @Thickness 0.0254 mm | 3680 psi @Thickness 0.00100 in |
Film Tensile Strength at Break, TD | 16.9 MPa @Thickness 0.0508 mm | 2450 psi @Thickness 0.00200 in |
| 17.3 MPa @Thickness 0.0254 mm | 2510 psi @Thickness 0.00100 in |
|
Thermal Properties | Metric | English | Comments |
---|
Melting Point | 112 °C | 234 °F |
Vicat Softening Point | 97.2 °C | 207 °F |
|
Optical Properties | Metric | English | Comments |
---|
Haze | 6.0 % @Thickness 0.0254 mm | 6.0 % @Thickness 0.00100 in |
| 7.0 % @Thickness 0.0508 mm | 7.0 % @Thickness 0.00200 in |
Gloss | 71 % @Thickness 0.0254 mm | 71 % @Thickness 0.00100 in |
| 76 % @Thickness 0.0508 mm | 76 % @Thickness 0.00200 in |
|
Processing Properties | Metric | English | Comments |
---|
Melt Temperature | 213 °C | 416 °F |
Blow-up Ratio (BUR) | 2.5 | 2.5 |
|
Descriptive Properties |
---|
Film Toughness | 666 ft-lb/in3 |
| 770 ft-lb/in3 |
| 780 ft-lb/in3 |
| 808 ft-lb/in3 |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.