MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
JSR Arton D4540 Cyclic Olefin Polymer
Categories: Polymer; Thermoplastic; Cyclo Olefin Polymer

Material Notes: ARTON has superior optical characteristics, dimensional stability, and high heat resistance. ARTON is used in optical applications such as optical films, light guiding plates, optical lenses etc. ARTON has a polar group in its molecular chain and has good adhesion, adherence, and miscibility.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.08 g/ccASTM D792
Water Absorption 0.20 %
@Time 605000 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.005 - 0.007 cm/cmASTM D955
Melt Flow 130 g/10 min
@Load 9.99 kg,
Temperature 260 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 125ASTM D785
Tensile Strength 60.0 MPa2 in/min (50 mm/min); ASTM D638
Elongation at Break 12 %2 in/min (50 mm/min); ASTM D638
Flexural Strength 120 MPa15 mm/min; ASTM D790
Flexural Modulus 2.65 GPa15 mm/min; ASTM D790
Izod Impact, Notched 30.0 J/m1/4 in notch; ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+16 ohm-cmASTM D257
Dielectric Constant 3.0
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 30.0 kV/mm
@Thickness 1.00 mm
ASTM D149
Dissipation Factor 0.020
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 190 sec
@Thickness 3.00 mm
ASTM D495
 
Thermal PropertiesOriginal ValueComments
CTE, linear 80.0 µm/m-°CASTM D696
Thermal Conductivity 0.180 W/m-K
@Temperature 100 °C
JSR Test
Deflection Temperature at 1.8 MPa (264 psi) 125 °CASTM D648
Glass Transition Temp, Tg 128 °CDSC, 20°C/min
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.515
@Wavelength 587.6 nm
d line; ASTM D542
Abbe Number 57
@Temperature 25.0 °C
ASTM D542
Haze 0.60 %
@Thickness 3.20 mm
ASTM D1003
Transmission, Visible 93 %
@Thickness 3.20 mm
ASTM D1003
 
Descriptive Properties
10% NaOH Resistance, 1 week at 23°CResistantASTM D543
10% Sulfuric Acid Resistance, 1 week at 23°CResistantASTM D543
Acetone Resistance, 1 week at 23°CResistantASTM D543
IPA Resistance, 1 week at 23°CLimited ResistanceASTM D543
MEK Resistance, 1 week at 23°CLimited ResistanceASTM D543
Methanol Resistance, 1 week at 23°CResistantASTM D543
Pencil HardnessHJIS K5401
Toluene Resistance, 1 week at 23°CNo ResistanceASTM D543

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultrason® E 1010 PES
JSR Arton F4520 Cyclic Olefin Polymer
BASF Ultrason® E 2010 HC PESU
Goodfellow TPX® DX350 Coating/Extrusion Grade Polymethylpentene
Polyplastics TOPAS® 5013F-04 Cyclic Olefin Copolymer (COC)

PJSRC991 / 191503

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.