MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay MTM® 49-3 Epoxy Prepreg with 36% M46J-124 Carbon Fiber
Categories: Polymer; Thermoset; Epoxy; Epoxy/Carbon Fiber Composite

Material Notes: MTM49-3 is an 80 to 160°C (176 to 320°F) curing, toughened epoxy pregpreg resin system developed specifically for the manufacture of components. MTM49-3 pregregs exhibit excellent ambient and hot mechanical performance combined with good impact resistance after only moderate cure cycles making them ideal for use in the motorsport industry.

Features & Benefits:

  • Autoclave and press curable
  • 60 days out life at 21°C (70°F)
  • 12 months storage at -18°C(0°F)
  • Versatile cure temperatures
  • 190°C Tg
  • Bonds directly to Nomex core in body type applications
Product Variants:
MTM49-3: High Tg and moderate toughness
MTM49-3B: Black pigmented variant of MTM49-3
MTM49-3BB: Black pigmented variant of MTM49-3 (higher pigment loading)
MTM49-3BD: Black dyed variant of MTM49-3

Property data reported for dry sample after cure cycle: 90 minutes at 135°C (275°F), 6.2 bar (90 psi). Data normalized to 55 vol% except for shear properties.

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.22 g/ccUnreinforced cured resin
Storage Temperature -18.0 °CResin
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 3740 psi90°; ASTM D3039
 248000 psi0°; ASTM D3039
Tensile Modulus 6.87 GPa90°; ASTM D3039
 235 GPa0°; ASTM D3039
Compressive Strength 189 MPa90°; SACMA SRM01R94
 875 MPa0°; SACMA SRM01R94
Compressive Modulus 7590 MPa90°; SACMA SRM01R94
 201000 MPa0°; SACMA SRM01R94
Shear Modulus 4.09 GPaIn-plane; ASTM D3518
Shear Strength 10000 psiIn-plane; ASTM D3518
 12800 psi0° Interlaminar; ASTM D2344
 
Thermal PropertiesOriginal ValueComments
Glass Transition Temp, Tg 95.0 °CDMA E' onset Tg, 16 hrs at 80°C, dry
 <= 115 °Cwet
 140 °CDMA E' onset Tg, 90 mins at 135°C, dry
 <= 190 °Cdry
 
Processing PropertiesOriginal ValueComments
Cure Time 1.00 hour
@Temperature 120 °C
Alternate Cure
 1.50 hour
@Temperature 135 °C
Recommended Cure
 4.00 hour
@Temperature 100 °C
Alternate Cure
 7.00 min
@Temperature 160 °C
Alternate Cure
 25.0 min
@Temperature 140 °C
Alternate Cure
Shelf Life 12.0 MonthResin

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay CYCOM® 2020 Epoxy + T800-6K 2X2T Twill 200 Prepreg, without Post-Cure
Solvay CYCOM® 977-6 Epoxy Laminate with IM7 Unidirectional Tape
Solvay MTM® 79 Epoxy Matrix with 50% CF1420 Carbon Fiber Composite
Solvay CYCOM® 950 Epoxy Prepreg with Hy-E Std/950 Unidirectional Tape and Roving
Hexcel® HexFlow® RTM 6 180°C Epoxy System for Resin Transfer Molding Monocomponent System

PCYTED146 / 180448

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.