MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

BASF Ultramid® A 218W V33 Natural T Nylon 66, 33% Glass Fiber Reinforced, Heat Stabilized
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled; Nylon 66, Heat Stabilized

Material Notes: Product Description: Ultramid® A 218W V33 Natural T is a polyamide 66, reinforced with 30% of glass fiber, heat stabilized, for injection molding. The product is particularly recommended for the molding of parts where some translucency is required, as well as surface aesthetics is important.

Availability: North America

Filler/Reinforcement: Glass Fiber, 33% Filler by Weight

Additive: Heat Stabilizer

Features: Good Dimensional Stability; Good Flow; Good Mold Release; Heat Stabilized - Organic

Use: Bobbins; Connectors

RoSH Compliance: RoSH Compliant

Appearance: Natural Color

Forms: Pellets

Processing Method: Injection Molding

Resin ID (ISO 1043): PA66-GF33

Information provided by BASF Corporation

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.40 g/cc0.0506 lb/in³ISO 1183
Maximum Moisture Content 0.200.20
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 19.0 MPa2760 psiISO 527-2
Elongation at Break 3.8 %3.8 %ISO 527-2
Tensile Modulus 10.2 GPa1480 ksiISO 527-1
Flexural Strength 294 MPa42600 psiISO 178
Flexural Modulus 8.96 GPa1300 ksiISO 178
Izod Impact, Notched (ISO) 11.3 kJ/m²5.40 ft-lb/in²ISO 180/A
Charpy Impact Unnotched 9.03 J/cm²43.0 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 1.09 J/cm²5.20 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 263 °C505 °FISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 263 °C505 °FUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 247 °C477 °FUnannealed; ISO 75-2/A
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 270 - 280 °C518 - 536 °F
Middle Barrel Temperature 275 - 285 °C527 - 545 °F
Front Barrel Temperature 280 - 290 °C536 - 554 °F
Mold Temperature 70.0 - 100 °C158 - 212 °F
Drying Temperature 80.0 °C176 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBASG2082 / 310775

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.