MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Murtfeldt Muralen® plus + AB Polyethylene, Antibacterial
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); UHMW PE (Ultra High Molecular Weight PE)

Material Notes: Muralen® is based on high molecular weight polyethylene (PE-HMW) and is ideally suited for use in applications that require the generally impressive material properties of polyethylene. Because of its great cut, impact, and shock resistance, this material is often used to make underlays for cutting and punching machines and for ram guards.

Special Properties:
• High cut resistance
• Good shock and impact absorption
• Good resistance to chemicals
• Good anti-adhesion properties
• Approved for use in the food industry (EU and FDA)
• Good weldability
• Antibacterial properties

Information provided by Murtfeldt Kunststoffe GmbH & Co. KG.

Key Words: PE-HMW
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density <= 0.950 g/ccISO 1183
Moisture Absorption at Equilibrium <= 0.10 %ISO 62
Water Absorption at Saturation <= 0.10 %ISO 62
Molecular Weight 500000 g/mol
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 66DIN 53505
Ball Indentation Hardness 45.0 MPa
Tensile Strength 27.2 MPaISO 527
Tensile Strength, Yield 20.0 MPaISO 527
Elongation at Break 630 %ISO 527
Modulus of Elasticity 1.10 GPa
Compressive Yield Strength 9.00 MPa
@Strain 1 %
ISO 604
 15.0 MPa
@Strain 2 %
ISO 604
 23.0 MPa
@Strain 5.0 %
ISO 604
Charpy Impact Unnotched NBISO 179
Charpy Impact, Notched >= 25.0 kJ/m²ISO 179
Coefficient of Friction, Dynamic 0.18
Sand Slurry 350value in %
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity >= 1.00e+14 ohm-cmIEC 60093
Surface Resistance >= 1.00e+13 ohmIEC 60093
Dielectric Constant 2.4
@Frequency 100 Hz
IEC 60250
 2.4
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength <= 45.0 kV/mmIEC 60243
Dielectric Loss Index 0.00020
@Frequency 100 Hz
IEC 60250
 0.00020
@Frequency 1e+6 Hz
IEC 60250
 
Thermal PropertiesOriginal ValueComments
CTE, linear 200 µm/m-°C
@Temperature 23.0 - 60.0 °C
Thermal Conductivity 0.400 W/m-KISO 52612
Melting Point 130 - 135 °CISO 3146
Maximum Service Temperature, Air 80.0 °C
@Time 1.80e+7 sec
Minimum Service Temperature, Air -100 °C
Glass Transition Temp, Tg -120 °C
Flammability, UL94 HB
 
Compliance PropertiesOriginal ValueComments
European Food 1935/2004 Yes
FDA Yes
 
Descriptive Properties
ColorSky Blue

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for High Density Polyethylene (HDPE), Injection Molded
Murtfeldt Original Material ”S”® plus + AB Polyethylene, Antibacterial
American Elements Z-MITE™ Zinc Oxide Nanopowder
Overview of materials for Linear Low Density Polyethylene (LLDPE), Rotational Molding Grade
Aclo Accutech Polyethylene HD0234G20UVL High Density Glass Reinforced UV Stabilized

PMURT918 / 156565

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.