MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AlphaGary Evoprene™ HP 3704 High Performance Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Styrenic TPE

Material Notes: Evoprene™ HP is a hydrogenated styrene block copolymer based thermoplastic elastomer. Specially formulated for applications requiring high strength and excellent abrasion resistance, Evoprene™ HP can be used in some applications where thermoplastic polyurethane would normally be specified.
Evoprene™ HP has very good, heat ageing properties, excellent hydrolysis resistance and, when properly protected, very good antimicrobial resistance.
Can be used in food contact applications with the appropriate stabilizer package

Alphagary is part of Orbia.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.890 g/ccISO 2782
Viscosity Measurement 19
@Temperature 150 °C
Kg/cm2; Macklow-Smith extrusion rheometer
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 50ISO 868
Tensile Strength 9.40 MPaISO 37
Elongation at Break 580 %ISO 37
100% Modulus 0.00180 GPa
@Strain 100 %
ISO 37
200% Modulus 0.00250 GPa
@Strain 200 %
ISO 37
300% Modulus 0.00300 GPa
@Strain 300 %
ISO 37
Tear Strength 41.0 kN/mISO 34-B
Abrasion 60mm3; DIN 53516
Compression Set 21 %
@Temperature 22.0 °C,
Time 259000 sec
ISO 815
 35 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815
 46 %
@Temperature 100 °C,
Time 79200 sec
ISO 815
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 125 °C
Minimum Service Temperature, Air -60.0 °C
 
Descriptive Properties
Bonds withPolypropylene
Chemical ResistanceAcetoneModerate/Good
 Acids up to 80%Excellent
 AlcoholExcellent
 AlkalisExcellent
 Brake fluidGood
 Chlorinate solventsPoor
 DieselPoor
 Ethylene glycolExcellent
 GasolinePoor
 Salt solutionExcellent
 Soda lyeExcellent
 Water, 23°CExcellent
 Water, 95°CGood

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Momentive Performance Materials Silopren™ LIM 6030 Liquid Silicone Rubber - Fast Cure / High Tear
Momentive Performance Materials Silopren™ LIM 6050 Liquid Silicone Rubber - Fast Cure / High Tear
Kraton® NEXAR™ MD9200 Polymer Barrier Membrane
Kraton® NEXAR™ MD9150 Polymer Barrier Membrane Solution
Kraton® NEXAR™ MD9150 Polymer Barrier Membrane

PGARY9644 / 140437

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.