MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI E4340 Steel, oil quenched 855°C (1570°F), 230°C (450°F) temper for 4hrs.
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 4000 Series Steel; Low Alloy Steel; Carbon Steel; Medium Carbon Steel

Material Notes: AISI E4340 has a favorable response to heat treatment (usually oil quenching followed by tempering) and exhibits a good combination of ductility and strength when treated thusly. Uses include piston pins, bearings, ordnance, gears, dies, and pressure vessels.

Key Words: alloy steels, UNS G43406, ASTM A304, ASTM A331, ASTM A505, ASTM A519
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.85 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Knoop 555Converted from Vickers hardness.
 572
@Temperature -78.0 °C
Converted from Vickers hardness
 666
@Temperature -195 °C
Converted from Vickers hardness
 851
@Temperature -255 °C
Converted from Vickers hardness
Hardness, Vickers 531
 548
@Temperature -78.0 °C
 639
@Temperature -195 °C
 818
@Temperature -255 °C
Tensile Strength, Ultimate 1855 MPa
 2020 MPa
@Temperature -78.0 °C
 2200 MPa
@Temperature -195 °C
 2290 MPa
@Temperature -255 °C
Tensile Strength, Yield 1550 MPa
 1915 MPa
@Temperature -195 °C
 1935 MPa
@Temperature -78.0 °C
Elongation at Break 12 %in 50 mm
 0.60 %
@Temperature -255 °C
in 50 mm
 10 %
@Temperature -195 °C
in 50 mm
 12 %
@Temperature -78.0 °C
in 50 mm
Reduction of Area 40 %
 0.20 %
@Temperature -255 °C
 24 %
@Temperature -195 °C
 40 %
@Temperature -78.0 °C
Modulus of Elasticity 196 GPa
 210 GPa
@Temperature -255 °C
 211 GPa
@Temperature -195 °C
 211 GPa
@Temperature -78.0 °C
Bulk Modulus 160 GPaTypical for steel.
Poissons Ratio 0.30Calculated
Machinability 50 %annealed and cold drawn. Based on 100% machinability for AISI 1212 steel.
Shear Modulus 75.0 GPaEstimated from elastic modulus
 81.0 GPa
@Temperature -255 °C
Estimated from elastic modulus
 81.0 GPa
@Temperature -195 °C
Estimated from elastic modulus
 81.0 GPa
@Temperature -78.0 °C
Estimated from elastic modulus
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000248 ohm-cm
@Temperature 20.0 °C
 0.0000298 ohm-cm
@Temperature 100 °C
 0.0000552 ohm-cm
@Temperature 400 °C
 0.0000797 ohm-cm
@Temperature 600 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.3 µm/m-°C
@Temperature 20.0 °C
 12.4 µm/m-°C
@Temperature 250 °C
 13.7 µm/m-°C
@Temperature 500 °C
Specific Heat Capacity 0.475 J/g-°CTypical 4000 series steel
Thermal Conductivity 44.5 W/m-KTypical steel
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.38 - 0.43 %
Chromium, Cr 0.70 - 0.90 %
Iron, Fe 95.175 - 96.27 %As remainder
Manganese, Mn 0.65 - 0.85 %
Molybdenum, Mo 0.20 - 0.30 %
Nickel, Ni 1.65 - 2.0 %
Phosphorus, P <= 0.025 %
Silicon, Si 0.15 - 0.30 %
Sulfur, S <= 0.020 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 4340 Steel, oil quenched 855°C (1570°F), 230°C (450°F) temper for 4 hrs.
AISI 4340 Steel, oil quenched 845°C, 425°C (800°F) temper
AISI E4340 Steel, heat treated, fatigue tested
AISI E4340 Steel, heat treated, nitrided for 48 hrs., fatigue tested
AISI E4340 Steel, heat treated, nitrided for 50 hrs., fatigue tested

M434DK / 7804

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.