MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Assab Steels VANADIS 4 Cold Work Steel
Categories: Metal; Ferrous Metal; Chrome-moly Steel; Tool Steel; Cold Work Steel

Material Notes: VANADIS 4 is a chromium-molybdenum-vanadium alloyed steel which is characterized by:
  • High wear resistance
  • High compressive strength
  • Very good through-hardening properties
  • Very good toughness
  • Excellent dimensional stability after hardening and tempering
  • Good resistance to tempering back

VANADIS 4 is especially suitable for applications where adhesive wear and/or chipping are the dominating problems, i.e.

  • with soft/adherent materials such as austenitic stainless steel, mild steel, copper, aluminum, etc. as work material
  • with thicker work material

Examples:
  • blanking and forming
  • Fine blanking
  • Cold extrusion tooling
  • Powder pressing
  • Deep drawing
  • Knives

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.273 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 55980°C Austenitizing temperature, for tempering at 300°C
 56.51000°C Austenitizing temperature, for tempering at 300°C
 581020°C Austenitizing temperature, for tempering at 300°C
 58.5980°C Austenitizing temperature, for tempering at 500°C
 59.5At 1000°C Austenitizing temperature
 59.51060°C Austenitizing temperature, for tempering at 300°C
 59.51000°C Austenitizing temperature, for tempering at 500°C
 60Hardened and tempered.
 611020°C Austenitizing temperature, for tempering at 500°C
 631060°C Austenitizing temperature, for tempering at 500°C
 63At 1040°C Austenitizing temperature
 64At 1080°C Austenitizing temperature
Modulus of Elasticity 200 GPa
 170 GPa
@Temperature 400 °C
Impact Test 50.0 Jtempering temperature of 500°C. Specimen size: 7x10x55 mm unnotched. Hardened at 1020°C. Quenched in air. Tempered twice
 83.5 Jtempering temperature of 275°C. Specimen size: 7x10x55 mm unnotched. Hardened at 1020°C. Quenched in air. Tempered twice
 95.0 Jtempering temperature of 600°C. Specimen size: 7x10x55 mm unnotched. Hardened at 1020°C. Quenched in air. Tempered twice
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.8 µm/m-°C
@Temperature 20.0 - 200 °C
 11.9 µm/m-°C
@Temperature 20.0 - 400 °C
Specific Heat Capacity 0.110 BTU/lb-°F
@Temperature 20.0 °C
Thermal Conductivity 26.0 W/m-K
@Temperature 20.0 °C
 27.0 W/m-K
@Temperature 200 °C
 28.5 W/m-K
@Temperature 400 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 1.5 %
Chromium, Cr 8.0 %
Iron, Fe 83.6 %
Manganese, Mn 0.40 %
Molybdenum, Mo 1.5 %
Silicon, Si 1.0 %
Vanadium, V 4.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 4140 Steel, normalized at 870°C (1600°F), air cooled, 13 mm (0.5 in.) round
Assab Steels VANADIS 4 EXTRA Cold Work Steel
Bohler-Uddeholm UDDEHOLM VANADIS 10 SUPERCLEAN 3 Powder Metallurgical Cold Work Tool Steel
Assab Steels ASP 23 Cold Work Steel
Assab Steels ASSAB 88 Cold Work Steel

NASSAB06 / 15024

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.