MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Ovako 18CrMo8-5* 225A Steel, Hardening
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: General Information: Ovako 225 is a steel specially designed for nitriding but is also suitable for carburizing or applications requiring quenched and tempered steels.
  • High nitriding rate
  • Suitable for nitriding, case carburizing or quench and tempering
  • Also suitable for applications require quenched and tempered steel in bars with diameter 25-160 mm.
  • Weldable under certain conditions
Variant 225A - Standard quality
Variant 225C - With a reduced sulphur content for a reduced number of sulphide inclusions

Information provided by Ovako

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell  255 - 320
@Thickness <=120 mm
255 - 320
@Thickness <=4.72 in
 265 - 320
@Thickness 80.0 - 120 mm
265 - 320
@Thickness 3.15 - 4.72 in
 265 - 320
@Thickness 80.0 - 120 mm
265 - 320
@Thickness 3.15 - 4.72 in
 275 - 330
@Thickness 80.0 mm
275 - 330
@Thickness 3.15 in
 275 - 330
@Thickness >=80.0 mm
275 - 330
@Thickness >=3.15 in
Tensile Strength  >= 840 MPa
@Thickness <=120 mm
>= 122000 psi
@Thickness <=4.72 in
 >= 860 MPa
@Thickness 80.0 - 120 mm
>= 125000 psi
@Thickness 3.15 - 4.72 in
 >= 860 MPa
@Thickness 80.0 - 120 mm
>= 125000 psi
@Thickness 3.15 - 4.72 in
 >= 880 MPa
@Thickness 80.0 mm
>= 128000 psi
@Thickness 3.15 in
 >= 880 MPa
@Thickness >=80.0 mm
>= 128000 psi
@Thickness >=3.15 in
Tensile Strength, Yield  >= 740 MPa
@Thickness <=120 mm
>= 107000 psi
@Thickness <=4.72 in
Reh
 >= 760 MPa
@Thickness 80.0 - 120 mm
>= 110000 psi
@Thickness 3.15 - 4.72 in
Reh
 >= 760 MPa
@Thickness 80.0 - 120 mm
>= 110000 psi
@Thickness 3.15 - 4.72 in
Reh
 >= 800 MPa
@Thickness 80.0 mm
>= 116000 psi
@Thickness 3.15 in
Reh
 >= 800 MPa
@Thickness >=80.0 mm
>= 116000 psi
@Thickness >=3.15 in
Reh
Elongation at Break  12 %
@Thickness 80.0 mm
12 %
@Thickness 3.15 in
 12 %
@Thickness >=80.0 mm
12 %
@Thickness >=3.15 in
 12 %
@Thickness 80.0 - 120 mm
12 %
@Thickness 3.15 - 4.72 in
 12 %
@Thickness 80.0 - 120 mm
12 %
@Thickness 3.15 - 4.72 in
 12 %
@Thickness <=120 mm
12 %
@Thickness <=4.72 in
Reduction of Area  55 %
@Thickness 80.0 mm
55 %
@Thickness 3.15 in
 55 %
@Thickness >=80.0 mm
55 %
@Thickness >=3.15 in
 55 %
@Thickness 80.0 - 120 mm
55 %
@Thickness 3.15 - 4.72 in
 55 %
@Thickness 80.0 - 120 mm
55 %
@Thickness 3.15 - 4.72 in
 55 %
@Thickness <=120 mm
55 %
@Thickness <=4.72 in
Modulus of Elasticity 210 GPa30500 ksi
Poissons Ratio 0.300.30
Shear Modulus 80.0 GPa11600 ksi
Impact Test  27.0 J
@Thickness 80.0 - 120 mm,
Temperature -20.0 °C
19.9 ft-lb
@Thickness 3.15 - 4.72 in,
Temperature -4.00 °F
 40.0 J
@Thickness <=120 mm,
Temperature 20.0 °C
29.5 ft-lb
@Thickness <=4.72 in,
Temperature 68.0 °F
 40.0 J
@Thickness >=80.0 mm,
Temperature -20.0 °C
29.5 ft-lb
@Thickness >=3.15 in,
Temperature -4.00 °F
 60.0 J
@Thickness 80.0 - 120 mm,
Temperature 20.0 °C
44.3 ft-lb
@Thickness 3.15 - 4.72 in,
Temperature 68.0 °F
 80.0 J
@Thickness 80.0 mm,
Temperature 20.0 °C
59.0 ft-lb
@Thickness 3.15 in,
Temperature 68.0 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
6.67 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
0.110 - 0.115 BTU/lb-°F
@Temperature 122 - 212 °F
Thermal Conductivity 40.0 - 45.0 W/m-K278 - 312 BTU-in/hr-ft²-°FAmbient temperature
Transformation Temperature 416 °C781 °FMS
 751 °C1380 °FAC1
 853 °C1570 °FAC3
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.16 - 0.19 %0.16 - 0.19 %
Chromium, Cr 1.75 - 2.0 %1.75 - 2.0 %
Iron, Fe 95.36 - 96.62 %95.36 - 96.62 %As Balance
Manganese, Mn 0.75 - 1.0 %0.75 - 1.0 %
Molybdenum, Mo 0.50 - 0.60 %0.50 - 0.60 %
Nickel, Ni <= 0.30 %<= 0.30 %
Phosphorus, P <= 0.020 %<= 0.020 %
Silicon, Si 0.20 - 0.40 %0.20 - 0.40 %
Sulfur, S 0.020 - 0.030 %0.020 - 0.030 %
Vanadium, V <= 0.10 %<= 0.10 %
 
Descriptive Properties
WeldabilityCEV 0.94max
 Pcm 0.42max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ATI Allegheny Ludlum Type AL 441HP™ Stainless Steel Alloy
ATI Allegheny Ludlum Stainless Steel Type 439/AL 439HP™ (ASTM XM-8; UNS S43035)
ATI Allegheny Ludlum AL 433™ Ferritic Stainless Steel, Annealed
Astralloy 4800® Wear Resistant Steel
ASTM A542/A542M Alloy Steel, Chromium Molybdenum

NOVAKO096 / 234395

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.