MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
SABIC SABIC® PP 651H PP (Global)
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: PP 651H is a high molecular weight, low melt flow rate polypropylene random copolymer (PP-R) green colored & specially designed for transport of hot and cold drinking water. This grade is highly heat stabilized and specially formulated for extraction resistance with improved throughput & gloss.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.897 g/ccASTM D1505
Melt Flow 0.25 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 0.40 g/10 min
@Load 5.00 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 93ASTM D785
Tensile Strength, Yield 28.0 MPaASTM D638
Elongation at Yield 13 %ISO 527-1/-2
Flexural Modulus, 1% Secant 900 MPaASTM D790 A
Izod Impact, Notched 220 J/mASTM D256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 80.0 °CBased on injection molded specimens.; ASTM D648
Vicat Softening Point 135 °CASTM D1525
 
Descriptive Properties
ColorNatural

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI11230 / 244697

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.