MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Type 332 Austenitic Stainless Steel, Hot rolled Pipe, UNS N08800
Categories: Metal; Ferrous Metal; Stainless Steel; T 300 Series Stainless Steel

Material Notes:

Information provided by Industeel, ATI, Carlson. and the references(s).

Key Words: ASTM B 409
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.027 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 550 MPa
Tensile Strength, Yield 240 MPa
Elongation at Break 25 %
Modulus of Elasticity 196 GPa
Poissons Ratio 0.34
Shear Modulus 73.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000990 ohm-cm
Magnetic Permeability 1.0092at 200 Oe
Curie Temperature -115 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 14.2 µm/m-°C
@Temperature 20.0 - 90.0 °C
 16.0 µm/m-°C
@Temperature 20.0 - 250 °C
 16.7 µm/m-°C
@Temperature 20.0 - 500 °C
Specific Heat Capacity 0.500 J/g-°C
Thermal Conductivity 11.6 W/m-K
Melting Point 1357 - 1385 °C
Solidus 1357 °C
Liquidus 1385 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.30 %
Carbon, C 0.030 %
Chromium, Cr 20.5 %
Copper, Cu 0.20 %
Iron, Fe 46 %as balance
Manganese, Mn 1.0 %
Nickel, Ni 31 %
Phosphorus, P 0.020 %
Silicon, Si 0.40 %
Sulfur, S 0.010 %
Titanium, Ti 0.30 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
X5CrNiMo17133 Austenitic Stainless Steel for medical instruments
AISI 1095 Steel, hot rolled, 19-32 mm (0.75-1.25 in) round
AISI 1116 Steel, hot rolled
AISI Type 651 (19-9) Stainless Steel cold rolled and stress relieved, 35 HRC hardness
ASTM A606 HSLA Steel, Cold Rolled Sheet

MQ332e / 172139

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.