MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Special Metals INCONEL® Alloy N06230 Ni-Cr-W-Mo Alloy
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: INCONEL® alloy N06230 is a carbide strengthened nickel-chromium-tungsten-molybdenum alloy with an exceptional combination of strength, stability, and resistance to corrosion at very high temperatures. Alloy N06230 offers particularly good resistance to oxidation at temperatures greater than 1800°F (980°C). It also offers good resistance to carburization and nitridation.

The alloy is nickel-based. Chromium imparts resistance to high temperature corrosion. Oxidation is further enhanced by a micro-addition of lanthanum. Tungsten and molybdenum in conjunction with the alloy's high carbon content are largely responsible for the strength of the alloy. The creep resistance is optimized by control of the boron content.

The combination of high temperature strength and resistance to creep, stress rupture, and corrosion make the alloy attractive for service at temperatures above 1800°F (980°C). Potential applications include equipment and components for land-based gas turbines, thermal and petrochemical processing, heat treating, and ore and metal refining.

Information Provided by Special Metals Corporation

Key Words: UNS N06230; W.Nr. 2.4733; ASTM B572; SAE/AMS 5891; ASTM B435; SAE/AMS 5878; ASTM B622; ASTM B619; ASTM B626; ASTM B366; ASTM B564; SAE/AMS 5839
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.91 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 12.0 ksi
@Temperature 1090 °C
Hot-Rolled/Annealed Plate
 34.0 ksi
@Temperature 871 °C
Hot-Rolled/Annealed Plate
 75.0 ksi
@Temperature 760 °C
Hot-Rolled/Annealed Plate
 105 ksi
@Temperature 538 °C
Hot-Rolled/Annealed Plate
 105 ksi
@Temperature 649 °C
Hot-Rolled/Annealed Plate
 108 ksi
@Temperature 427 °C
Hot-Rolled/Annealed Plate
 110 ksi
@Temperature 316 °C
Hot-Rolled/Annealed Plate
 112 ksi
@Temperature 204 °C
Hot-Rolled/Annealed Plate
 117 - 122 ksi
@Temperature 21.1 °C
Hot-Rolled/Annealed Plate - Typical Range
Tensile Strength, Yield 8.00 ksi
@Strain 0.2 %,
Temperature 1090 °C
Hot-Rolled/Annealed Plate
 28.0 ksi
@Strain 0.2 %,
Temperature 871 °C
Hot-Rolled/Annealed Plate
 42.0 ksi
@Strain 0.2 %,
Temperature 649 °C
Hot-Rolled/Annealed Plate
 42.0 ksi
@Strain 0.2 %,
Temperature 760 °C
Hot-Rolled/Annealed Plate
 45.0 ksi
@Strain 0.2 %,
Temperature 538 °C
Hot-Rolled/Annealed Plate
 52.0 ksi
@Strain 0.2 %,
Temperature 427 °C
Hot-Rolled/Annealed Plate
 54.0 ksi
@Strain 0.2 %,
Temperature 316 °C
Hot-Rolled/Annealed Plate
 56.0 ksi
@Strain 0.2 %,
Temperature 204 °C
Hot-Rolled/Annealed Plate
 55.0 - 62.0 ksi
@Strain 0.2 %,
Temperature 21.1 °C
Hot-Rolled/Annealed Plate - Typical Range
Elongation at Break 40 %
@Temperature 538 °C
Hot-Rolled/Annealed Plate
 45 %
@Temperature 204 °C
Hot-Rolled/Annealed Plate
 46 %
@Temperature 316 °C
Hot-Rolled/Annealed Plate
 44 - 48 %
@Temperature 21.1 °C
Hot-Rolled/Annealed Plate - Typical Range
 48 %
@Temperature 427 °C
Hot-Rolled/Annealed Plate
 50 %
@Temperature 649 °C
Hot-Rolled/Annealed Plate
 70 %
@Temperature 760 °C
Hot-Rolled/Annealed Plate
 70 %
@Temperature 1090 °C
Hot-Rolled/Annealed Plate
 90 %
@Temperature 871 °C
Hot-Rolled/Annealed Plate
Rupture Strength 9000 psi
@Temperature 927 °C,
Time 270000 sec
Modulus of Elasticity 167 GPa
@Temperature 800 °C
 175 GPa
@Temperature 700 °C
 183 GPa
@Temperature 600 °C
 188 GPa
@Temperature 500 °C
 194 GPa
@Temperature 400 °C
 199 GPa
@Temperature 300 °C
 203 GPa
@Temperature 200 °C
 208 GPa
@Temperature 100 °C
 212 GPa
@Temperature 22.0 °C
Poissons Ratio 0.31
@Temperature 700 °C
 0.32
@Temperature 500 °C
 0.33
@Temperature 100 °C
 0.33
@Temperature 800 °C
 0.34
@Temperature 400 °C
 0.34
@Temperature 200 °C
 0.34
@Temperature 600 °C
 0.34
@Temperature 22.0 °C
 0.35
@Temperature 300 °C
Shear Modulus 63.0 GPa
@Temperature 800 °C
 67.0 GPa
@Temperature 700 °C
 68.0 GPa
@Temperature 600 °C
 71.0 GPa
@Temperature 500 °C
 73.0 GPa
@Temperature 400 °C
 74.0 GPa
@Temperature 300 °C
 76.0 GPa
@Temperature 200 °C
 78.0 GPa
@Temperature 100 °C
 79.0 GPa
@Temperature 22.0 °C
Charpy Impact, Notched 74.6 - 81.3 J/cm²V Notch 10 x 5 mm; Hot-Rolled/Annealed Plate; Longitudinal
 74.6 - 81.3 J/cm²V Notch 10 x 5 mm; Hot-Rolled/Annealed Plate; Transverse
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00012625 ohm-cm
@Temperature 22.0 °C
 0.00012643 ohm-cm
@Temperature 100 °C
 0.00012775 ohm-cm
@Temperature 200 °C
 0.00012849 ohm-cm
@Temperature 300 °C
 0.00012994 ohm-cm
@Temperature 900 °C
 0.00012994 ohm-cm
@Temperature 1000 °C
 0.00013085 ohm-cm
@Temperature 800 °C
 0.0001314 ohm-cm
@Temperature 400 °C
 0.00013217 ohm-cm
@Temperature 700 °C
 0.00013274 ohm-cm
@Temperature 500 °C
 0.00013343 ohm-cm
@Temperature 600 °C
Magnetic Permeability 1.002
@Temperature 21.0 °C
200 Oersted
 
Thermal PropertiesOriginal ValueComments
CTE, linear 3.84 µm/m-°C
@Temperature 100 °C
 3.88 µm/m-°C
@Temperature 200 °C
 3.99 µm/m-°C
@Temperature 300 °C
 4.11 µm/m-°C
@Temperature 400 °C
 4.18 µm/m-°C
@Temperature 500 °C
 4.23 µm/m-°C
@Temperature 600 °C
 4.28 µm/m-°C
@Temperature 700 °C
 4.47 µm/m-°C
@Temperature 800 °C
 4.62 µm/m-°C
@Temperature 900 °C
Melting Point 1360 - 1410 °C
Solidus 1360 °C
Liquidus 1410 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.20 - 0.50 %
Boron, B <= 0.015 %
Carbon, C 0.050 - 0.15 %
Chromium, Cr 20 - 24 %
Cobalt, Co <= 5.0 %
Iron, Fe <= 3.0 %
Lanthanum, La 0.0050 - 0.050 %
Manganese, Mn 0.30 - 1.0 %
Molybdenum, Mo 1.0 - 3.0 %
Nickel, Ni 47.49 - 65.195 %Balance
Phosphorus, P <= 0.030 %
Silicon, Si 0.25 - 0.75 %
Sulfur, S <= 0.015 %
Tungsten, W 13 - 15 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
MetalTek HAYNES® 230 Severe Corrosion and Heat Resistant Alloy
Alloy Wire International RW 80 Ni-Cr Resistance Wire
440A Martensitic Stainless Steel (UNS S44002)
444 Ferritic Stainless Steel, 18Cr-2Mo (UNS S44400)
Special Metals INCONEL® alloy MA758 Ni-Cr Superalloy

NINDA05 / 98896

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.