MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Mocom (ALBIS) ALFATER XL® A50I 2GP0050 PP/EPDM
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Base Polymer: Thermoplastic Vulcanisate PP/EPDM-Elastomer

Special Features: Injection molding grade, good weathering resistance, resistant to alkalis, resistant to ozone, resistant to hot air

Market Segment: Automotive, Building and Construction, Various

Application Area: Various

Typical Application: Seals, handles, tool handles, furniture handles/ knobs, racking/shelving, impact protection/shock absorber, buffer, gear stick, knob, protection cap, various

Information provided by Albis Plastics

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.950 g/cc0.0343 lb/in³ISO 1183
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 50
@Time 15.0 sec
50
@Time 0.00417 hour
ISO 868
Tensile Strength 4.60 MPa667 psitype 2; ISO 37
Tensile Stress at Strain 1.80 MPa
@Strain 100 %
261 psi
@Strain 100 %
type 2; ISO 37
Elongation at Break 340 %340 %type 2; ISO 37
Tear Strength 18.0 kN/m103 plimethod Ba; ISO 34-1
Compression Set 32 %
@Temperature 100 °C,
Time 79200 sec
32 %
@Temperature 212 °F,
Time 22.0 hour
25% Type A; ISO 815
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 125 °C257 °F
Minimum Service Temperature, Air -40.0 °C-40.0 °F
 
Processing PropertiesMetricEnglishComments
Melt Temperature 195 - 215 °C383 - 419 °FInjection molding
Mold Temperature 10.0 - 70.0 °C50.0 - 158 °FInjection molding
Drying Temperature 70.0 - 80.0 °C
@Time 7200 - 14400 sec
158 - 176 °F
@Time 2.00 - 4.00 hour
in a dry air (desiccant) dryer
 
Descriptive Properties
Base PolymerThermoplastic Vulcanizate PP/EPDM-Elastomer

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PALBIS8583 / 242642

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.