MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LEXAN™ Copolymer EXL4019 Polycarbonate (PC) (Asia)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LEXAN EXL4019 is an opaque 9% Glass Fiber (GF) reinforced polycarbonate (PC) siloxane copolymer resin for injection molding (IM) applications requiring improved stiffness. This resin also offers improved ductility over conventional GF reinforced PC resins in combination with medium flow characteristics and excellent processability with opportunities for shorter IM cycle times when compared to standard PC. LEXAN EXL4019 resin is a product that may be an excellent candidate for a wide variety of applications. Available in limited colors only.

Features: High Impact Resistance

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.25 g/cc1.25 g/ccASTM D792
Density 1.25 g/cc0.0452 lb/in³ISO 1183
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.400 %0.400 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.15 %0.15 %ISO 62-1
Viscosity 6.0 cP
@Load 1.20 kg,
Temperature 300 °C
6.0 cP
@Load 2.65 lb,
Temperature 572 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0020 - 0.0060 cm/cm
@Thickness 3.20 mm
0.0020 - 0.0060 in/in
@Thickness 0.126 in
SABIC method
Linear Mold Shrinkage, Transverse 0.0020 - 0.0060 cm/cm
@Thickness 3.20 mm
0.0020 - 0.0060 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 7.5 g/10 min
@Load 1.20 kg,
Temperature 300 °C
7.5 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 45.0 MPa6530 psi5 mm/min; ASTM D638
 48.0 MPa6960 psi5 mm/min; ISO 527
Tensile Strength, Yield 54.0 MPa7830 psi5 mm/min; ISO 527
 55.0 MPa7980 psi5 mm/min; ASTM D638
Elongation at Break 8.7 %8.7 %5 mm/min; ISO 527
 14 %14 %5 mm/min; ASTM D638
Elongation at Yield 4.3 %4.3 %5 mm/min; ASTM D638
 4.3 %4.3 %5 mm/min; ISO 527
Tensile Modulus 3.90 GPa566 ksi1 mm/min; ISO 527
 3.95 GPa573 ksi5 mm/min; ASTM D638
Flexural Strength 98.0 MPa14200 psiyield, 2 mm/min; ISO 178
 103 MPa14900 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 3.45 GPa500 ksi2 mm/min; ISO 178
 3.50 GPa508 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 345 J254 ft-lbASTM D256
 150 J
@Temperature -30.0 °C
111 ft-lb
@Temperature -22.0 °F
ASTM D256
Izod Impact, Notched (ISO) 25.0 kJ/m²11.9 ft-lb/in²80*10*3; ISO 180/1A
 10.0 kJ/m²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
80*10*3; ISO 180/1A
Izod Impact, Unnotched (ISO) NBNB80*10*3; ISO 180/1U
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
80*10*3; ISO 180/1U
Charpy Impact Unnotched NBNBEdgew 80*10*3 sp=62mm; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Edgew 80*10*3 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 2.50 J/cm²11.9 ft-lb/in²Edgew 80*10*3 sp=62mm; ISO 179/1eA
 1.50 J/cm²
@Temperature -30.0 °C
7.14 ft-lb/in²
@Temperature -22.0 °F
Edgew 80*10*3 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 40.0 J29.5 ft-lbASTM D3763
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  47.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
26.1 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 47.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
26.1 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow  70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Hot Ball Pressure Test 75.0 °C167 °FPASS; IEC 60695-10-2
Deflection Temperature at 1.8 MPa (264 psi) 135 °C275 °FEdgew 120*10*4 sp=100mm; ISO 75/Ae
 137 °C
@Thickness 3.20 mm
279 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 146 °C295 °FRate B/50; ASTM D1525
 146 °C295 °FRate B/120; ISO 306
 146 °C295 °FRate B/50; ISO 306
UL RTI, Electrical 80.0 °C176 °FUL 746B
UL RTI, Mechanical with Impact 80.0 °C176 °FUL 746B
UL RTI, Mechanical without Impact 80.0 °C176 °FUL 746B
Flammability, UL94 HB
@Thickness >=0.750 mm
HB
@Thickness >=0.0295 in
UL 94
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 305 - 325 °C581 - 617 °F
Zone 2 300 - 320 °C572 - 608 °F
Zone 3 310 - 330 °C590 - 626 °F
Melt Temperature 310 - 330 °C590 - 626 °FInjection Molding
Mold Temperature 80.0 - 115 °C176 - 239 °F
Drying Temperature 120 °C248 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
 48.0 hour48.0 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 40 - 60 %40 - 60 %
Vent Depth 0.00250 - 0.00760 cm0.000984 - 0.00299 in
Screw Speed 40 - 70 rpm40 - 70 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH80195 / 288142

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.