MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Hexcel® HexPly® M12 135°C Curing Epoxy Matrix, TVR380/26% Fiber
Categories: Polymer; Thermoset; Epoxy; Epoxy Cure Resin

Material Notes:

Information provided by HexCel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.24 g/cc0.0448 lb/in³Resin Density
 2.56 g/cc0.0925 lb/in³Fiber Density
Filler Content 60.0 %60.0 %Fiber Volume
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 55.0 MPa7980 psi90º, RT, Dry; EN2561
 1560 MPa226000 psiRT; Dry; EN2561
 16.0 MPa
@Temperature 100 °C
2320 psi
@Temperature 212 °F
90º, Wet; EN2561
 23.0 MPa
@Temperature 75.0 °C
3340 psi
@Temperature 167 °F
90º, Wet; EN2561
 620 MPa
@Temperature 100 °C
89900 psi
@Temperature 212 °F
Wet; EN2561
 670 MPa
@Temperature 75.0 °C
97200 psi
@Temperature 167 °F
Wet; EN2561
Tensile Modulus 16.0 GPa2320 ksi90º, RT, Dry; EN2561
 56.0 GPa8120 ksiRT; Dry; EN2561
 8.00 GPa
@Temperature 100 °C
1160 ksi
@Temperature 212 °F
90º, Wet; EN2561
 11.0 GPa
@Temperature 75.0 °C
1600 ksi
@Temperature 167 °F
90º, Wet; EN2561
 50.0 GPa
@Temperature 100 °C
7250 ksi
@Temperature 212 °F
Wet; EN2561
 51.0 GPa
@Temperature 75.0 °C
7400 ksi
@Temperature 167 °F
Wet; EN2561
Compressive Yield Strength 130 MPa18900 psiRT; Dry; DIN65380
 214 MPa31000 psi90º, RT, Dry; DIN65380
 140 MPa
@Temperature 100 °C
20300 psi
@Temperature 212 °F
90º, Wet; DIN65380
 165 MPa
@Temperature 75.0 °C
23900 psi
@Temperature 167 °F
90º, Wet; DIN65380
 800 MPa
@Temperature 100 °C
116000 psi
@Temperature 212 °F
Wet; DIN65380
 850 MPa
@Temperature 75.0 °C
123000 psi
@Temperature 167 °F
Wet; DIN65380
Compressive Modulus 16.5 GPa2390 ksi90º, RT, Dry; DIN65380
 58.0 GPa8410 ksiRT; Dry; DIN65380
 12.0 GPa
@Temperature 100 °C
1740 ksi
@Temperature 212 °F
90º, Wet; DIN65380
 13.5 GPa
@Temperature 75.0 °C
1960 ksi
@Temperature 167 °F
90º, Wet; DIN65380
 52.0 GPa
@Temperature 100 °C
7540 ksi
@Temperature 212 °F
Wet; DIN65380
 53.0 GPa
@Temperature 75.0 °C
7690 ksi
@Temperature 167 °F
Wet; DIN65380
Shear Strength 67.0 MPa9720 psiIn-Plane, RT, Dry; EN6031
 95.0 MPa13800 psi0º, ILSS (Short Beam), RT, Dry; EN2563
 45.0 MPa
@Temperature 100 °C
6530 psi
@Temperature 212 °F
0º, ILSS (Short Beam), Wet; EN2563
 45.0 MPa
@Temperature 100 °C
6530 psi
@Temperature 212 °F
In-Plane, Wet; EN6031
 52.0 MPa
@Temperature 75.0 °C
7540 psi
@Temperature 167 °F
In-Plane, Wet; EN6031
 61.0 MPa
@Temperature 75.0 °C
8850 psi
@Temperature 167 °F
0º, ILSS (Short Beam), Wet; EN2563
 
Processing PropertiesMetricEnglishComments
Shelf Life 14.0 Month
@Temperature -18.0 °C
14.0 Month
@Temperature -0.400 °F
 
Descriptive Properties
Cured Thickness per Ply (cm)0.25

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Hexcel® HexPly® M12 135°C Curing Epoxy Matrix, 37%/7781 Fiber
Hexcel® HexPly® M12 135°C Curing Epoxy Matrix, 45% 46280 Fiber
Hexcel® HexPly® M34 75°C (167°F) Curing Epoxy Matrix, High Strength 12k Carbon Balanced Fabric 600 g/m2
BorsodChem ONGRO CPE 4002 N Chlorinated Polyethylene
BorsodChem ONGRO CPE 3602 C Chlorinated Polyethylene

PHEXC158 / 98628

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.